Meaning
Measurement temperature is the temperature at which a machined plastic part is measured and at which its drawn dimensions are taken to apply. For metal a few kelvin barely matter. For plastic the same few kelvin can use up most of a tolerance. A plastic dimension is therefore a number plus a temperature, and both belong on the drawing and on the report.Reference Choice
Two temperatures are in play. Industrial lengths have been defined at 20 °C (68 °F) since 1931. Data sheets, such as Mitsubishi’s, state their values at 23 °C (73 °F). A drawing that cites a property from a sheet and a dimension under the metrology convention quotes two temperatures 3 K (5.4 °F) apart. The drawing picks one and uses it on every feature.Read More
Size Change per Kelvin
The gap matters because plastics expand so much. Over those 3 K, a 100 mm (3.94 in) feature changes by 0.059 mm (0.0023 in) in UHMW-PE. Acetal homopolymer changes by 0.037 mm (0.0014 in) and HDPE by 0.032 mm (0.0013 in). Cast acrylic moves 0.021 mm (0.0008 in) and unfilled PEI 0.017 mm (0.0007 in). Glass-filled PEI moves only 0.006 mm (0.0002 in). These figures are arithmetic on each grade’s published coefficient.Tolerance Budget
Turned backward, the same coefficients say how many kelvin a tolerance can absorb. A band of 0.05 mm (0.002 in) on a 100 mm (3.94 in) feature is used up by 2.5 K (4.5 °F) in UHMW-PE. Acetal uses it up in 4.1 K (7.4 °F) and HDPE in 4.6 K (8.3 °F). Unfilled PEI takes 9.0 K (16.2 °F), glass-filled PEI 25 K (45 °F) and steel about 42 K (75 °F). A workshop that drifts 6 K (11 °F) during a day moves a 100 mm acetal feature by 0.073 mm (0.0029 in). That is 81 percent of Mitsubishi’s best published acetal figure of 0.09 mm (0.0035 in) at that size. The same 6 K (11 °F) drift moves a 100 mm (3.94 in) HDPE feature by 0.065 mm (0.0026 in). That is 43 percent of the published HDPE best of 0.15 mm (0.0059 in). Unfilled PEI moves 0.034 mm (0.0013 in), 56 percent of its 0.06 mm (0.0024 in). The shares are rough, because the guide does not say whether its figures are bands or plus-and-minus values. The same tolerance line means very different things for two materials. A fit that has to hold across a range of room or service temperatures favors grades with low coefficients. At 20 x 10⁻⁶ per K, 30 percent glass-filled PEI sits within 1.7 times the steel figure that NIST gives. Unfilled acetal sits at about 10 times. Where the grade is fixed, the measurement temperature and the soak carry the burden instead.Warm-Part Error
Heat from the cut leaves a fresh part warm, so a first reading at the machine reads large. Stress released by the cut shifts the part over hours, and moisture changes it over days to weeks. Mitsubishi’s turning tips advise roughing, a rest of 24 hours and a final cut, and aiming for the lowest dimension because most diameters grow. A first-article measurement taken warm and fresh is not the size the part keeps. One taken after the rest, at the stated temperature, is.Drawing Line
The sources suggest a threshold for the note. The PEI article asks for a measurement temperature and humidity condition on any dimension under about 0.1 mm (0.004 in). The polyethylene article sets the line at about 0.2 mm (0.008 in), because its expansion is larger. A hole call-out on any plastic adds the measurement temperature and a rest time after machining. A model line reads: dimensions at 20 °C (68 °F) after 24 hours at that temperature.Report Content
Mitsubishi advises capability studies on a shop’s own machines, because its table is a best case. Such a study only means something if every part is measured at a stated temperature after a stated rest. A spread measured warm on some parts and cold on others measures the room as much as the process. An inspection record carries the measurement temperature and the soak time beside the results. That lets an incoming inspection reproduce the reading. It also lets a later batch be compared with the first without guessing at the room. A disagreement of a few hundredths of a millimeter can then be traced to its source.