AcetalAcrylicStock Shape

Drilling Deep Holes in Plastic Without Melting or Cracking

Holes deeper than two diameters trap heat in plastic, so drill grind, peck cycle, coolant choice and cool-down decide whether the part cracks or holds its size.

A CNC machined natural cream nylon block cut in half along a long drilled hole, the clean bore wall showing, beside a long thin twist drill.

A 60 mm (2.4 in) bar of reinforced plastic that needs a deep bore may spend six hours in an oven before the drill touches it. Ensinger, a maker of engineering plastic stock shapes, suggests drilling such parts pre-warmed to about 120 °C (248 °F) and allows roughly one hour of heating per 10 mm (0.39 in) of cross-section. The oven is not there to soften the cut. It is there because a cold, stiff blank with a hot hole in its center can split along its axis.

That failure explains the whole operation. Plastic conducts heat poorly, so the energy of a deep hole stays in the hole. The wall swells, the swelling pushes against cooler material around it, and the stress that results can crack the blank or leave the finished part out of shape days later. What follows tracks a deep hole from the drill grind to the drawing note, with the figures the stock makers print.

How to Drill a Deep Hole in Plastic Without Melting or Cracking

Treat any hole deeper than two diameters as a cooling problem first and a cutting problem second. Both Mitsubishi Chemical Advanced Materials (MCAM) and Ensinger name the same threshold: heat builds very easily once the depth passes twice the diameter. From there the makers’ advice converges on a short sequence.

  1. Use a sharp drill with a thinned or narrow web and a slow helix, so it cuts instead of rubbing and lifts chips out of the flutes.
  2. Withdraw the drill often (peck drilling) to clear chips and let the hole cool.
  3. Apply coolant, compressed air or a spray mist; deep holes are one of the few plastic operations where Ensinger names coolant as the rule rather than the exception.
  4. Open large diameters in stages and finish them with a boring tool.
  5. Drill long rods from one end only, and pre-warm thick or reinforced blanks when the makers advise it.
  6. Let the part cool completely before the finishing cut or the measurement.

None of these steps is exotic. The difficulty is that skipping any one of them shows up late, as a crack found at inspection or a bore that has moved after the part was released.

A deep hole in plastic fails by heat that cannot leave. Every rule for drilling one either removes heat with the chip, removes it with coolant, or stops it from building in the first place.

Why Depth Past Two Diameters Changes the Job

Near the surface, a drill in plastic behaves much as it does in aluminum. Chips leave freely, air reaches the cutting edges, and most of the heat goes out with the swarf. Below two diameters the flutes fill, the chips start to rub on the hole wall, and the cutting zone loses its exit.

Tangram Technology, a UK plastics engineering consultancy, calls drilling the most problematic machining operation for plastics because it joins concentrated heat with chip congestion in a confined space. Its guide lists the results in order of severity: smearing, local melting, internal stress, cracking and dimensional error. Ensinger’s answer to the same question adds that semi-crystalline plastics such as acetal, nylon and PEEK are especially prone, because they build heat quickly while drilling.

The mechanism behind the cracks is worth stating plainly. Ensinger describes internal expansion in the component as the hole heats, which puts the surrounding material under compressive stress. The effect is strongest when drilling into the center of round rod. If the stress is high enough, the blank warps, loses its dimensions, fractures or bursts open.

Stock shapes start with some stress of their own. Ensinger explains that extruded rods and plates cool from the outside inward, so the core is held by an already rigid skin as it shrinks. A drill that heats that core is working in the region where the stock is already most loaded.

Where Melting Starts

Melting starts where a cutting edge stops cutting. A dull drill, a heel that rubs because the relief is too small, or a feed so light that the edge skates on the material will each turn cutting energy into friction. Tangram’s guide states the principle for all plastic operations: light cuts that rub create more heat than properly loaded cuts. A drill that is fed too gently into a deep hole is the classic case.

Drill Geometry for Plastic Stock

Standard high-speed steel (HSS) twist drills work in most unfilled plastics, but the makers adjust the grind. Table 1 sets their published values side by side. The acrylic column comes from Röhm, the maker of PLEXIGLAS, whose figures differ most from a metal-cutting drill because acrylic chips at the hole exit if the drill cuts aggressively.

Table 1. Drill geometry published by three plastic stock makers
Feature MCAM 2026, most stock-shape families Ensinger FAQ, holes under 25 mm (0.98 in) Röhm, PLEXIGLAS GS and XT
Point angle 90 to 120° Not stated 60 to 90°
Relief (clearance) angle 5 to 10° Not stated 3 to 8°
Rake angle 3 to 5° Neutral 0° for thin-walled parts 0 to 4°
Helix or twist angle Slow spiral (low helix) 12 to 25° 12 to 16°
Web Thinned web on larger drills Narrow bridge Thin the transverse edge above about 8 mm (0.31 in)
Tool material HSS or carbide; carbide, PCD or CVD for reinforced grades Well-sharpened HSS Reground HSS

Two points in the table carry most of the weight for deep holes. The low helix gives wide, smooth flutes that lift chips instead of packing them. A thinned web shrinks the rubbing zone at the drill’s center, where cutting speed falls toward zero and friction does most of the work.

Reinforced grades change the tool material, not the logic. MCAM moves glass-filled and carbon-filled PEEK, PAI and PPS to carbide or diamond (PCD or CVD) drills, and Ensinger warns that hardened steel tools wear out too fast on these materials. Ensinger also notes that it grinds special tools such as step drills in its own tool shop for specific plastic parts, which is a reminder that a deep, precise hole in a demanding grade is often worth a dedicated drill.

Speeds, Feeds and the Peck Cycle

MCAM prints drilling data by material family. For nylon, UHMW-PE and acetal it gives a cutting speed of 50 to 100 m/min (164 to 328 ft/min) at a feed of 0.1 to 0.3 mm/rev (0.004 to 0.012 in/rev). Unfilled PEEK and PET-P drop to 50 to 80 m/min (164 to 262 ft/min) with carbide, as do the glass- and carbon-filled grades with carbide or diamond drills, and PBI and PI fall to 25 to 50 m/min (82 to 164 ft/min). Tangram’s table gives the same 50 to 100 m/min and 0.1 to 0.3 mm/rev for nylon and acetal.

A cutting speed becomes a spindle speed only through the drill diameter. Tangram prints the conversion: spindle speed equals 1,000 times the cutting speed divided by pi times the diameter in millimeters. Table 2 applies it at the bottom of MCAM’s range, 50 m/min, which is the speed common to every unfilled family in the guide.

Table 2. Spindle speed and feed rate at 50 m/min (164 ft/min), computed from the MCAM drilling range and the Tangram conversion
Drill diameter, mm (in) Spindle speed, rpm Feed rate at 0.1 mm/rev, mm/min (in/min) Feed rate at 0.3 mm/rev, mm/min (in/min)
3 (0.12) 5,305 531 (20.9) 1,592 (62.7)
6 (0.24) 2,653 265 (10.4) 796 (31.3)
10 (0.39) 1,592 159 (6.3) 477 (18.8)
16 (0.63) 995 99 (3.9) 298 (11.7)
25 (0.98) 637 64 (2.5) 191 (7.5)

The table shows why small deep holes are the risky ones. A 3 mm drill needs more than 5,000 rpm to reach even the low end of the speed range, while its flutes are tiny and fill within a few millimeters of depth.

Feed deserves the same care as speed. Röhm’s drilling photographs make the point visually for acrylic: a speed or feed that is too high gives a crumbly chip and an uneven wall, while one that is too slow gives a molten chip and signs of decomposition in the hole. The right pair gives a smooth, continuous chip. At a 25 mm (0.98 in) diameter and 0.1 to 0.3 mm/rev, Röhm names 510 rpm as the most favorable speed in its chart.

Setting the Peck Depth

No maker document in this set prints a peck depth. MCAM calls frequent pull-outs necessary for heat and swarf removal in holes from 0.5 to 25 mm (0.02 to 0.98 in). Ensinger asks for frequent withdrawal of the drill for chip removal and extra cooling. Röhm says that thick material, deep holes and blind holes drilled by hand should be lifted several times.

The interval is therefore found on the first parts: watch the chip, feel for a temperature rise in the part, and shorten the peck until the chip stays continuous to full depth.

Ensinger adds one rule that matters on manual machines. It advises against hand feed for drilling, so the drill cannot grab and crack the part.

Coolant and Chip Removal in a Deep Hole

Dry machining is the trend in plastics, and Ensinger says most operations can now run without cutting fluid. It then names three exceptions: deep drill holes, thread cutting and sawing of reinforced materials. MCAM gives the same exception in different words, recommending a cooling liquid for drilling because heat builds so easily once the depth passes twice the diameter.

The choice of fluid depends on the polymer. MCAM suggests nonaromatic, water-soluble coolants and warns that mineral-oil cutting fluids can contribute to stress cracking in amorphous plastics such as polycarbonate, PPSU, PEI and PSU. If coolant is used on those materials, MCAM asks for an immediate wash in isopropyl alcohol and pure water after machining. Ensinger gives the same rinse and lists pure water or compressed air as the safer media for amorphous grades.

Some grades take no liquid at all. MCAM marks its flame-retardant TIVAR BurnGuard UHMW-PE as dry machining only, because the flame-retardant additives can react with water- or oil-based coolants and corrode steel machine parts and tooling. Compressed air or an air spray is the only cooling it allows. For acrylic, Röhm asks for a cooling lubricant or an acrylic-compatible drilling emulsion from a material thickness of 5 mm (0.20 in) onward, and for emulsion only in deep holes.

Coolant in a deep plastic hole is chosen by the polymer, not the machine. Water-based media or air suit most grades, mineral oil can crack amorphous ones, and some flame-retardant grades take nothing wet at all.

Large Diameters by Stages and Boring

Above 25 mm (0.98 in) the makers stop treating a hole as a single drilling operation. MCAM’s example is a 50 mm (1.97 in) bore made by drilling successively with 12 mm (0.47 in) and 25 mm (0.98 in) drills, then opening the hole further with larger drills or a single boring tool. Ensinger sets a similar ceiling: a pre-drilled diameter no larger than 25 mm, then finishing with an internal cutting tool. Tangram lists staged opening of large holes and boring instead of drilling for sensitive materials among its best practices.

Ensinger adds three rules for long rods. Drill from one side only, because two holes started from opposite ends that meet in the middle create unfavorable stress and can tear the part. In extreme cases, and for reinforced grades, drill a pre-warmed blank at about 120 °C (248 °F). Then finish-machine only after the blank has cooled completely, so the final dimensions are cut on a part at room temperature.

For unreinforced nylons Ensinger gives a separate pre-heating band of 80 to 120 °C (176 to 248 °F) for large stock, which it defines as round rods above 100 mm (3.9 in) diameter and plates above 80 mm (3.1 in) thick. The purpose is the same: to keep the drill from cracking a blank whose core is drier and harder than its skin. Table 3 converts Ensinger’s heating allowance into oven time.

Table 3. Pre-warming time for drilling, computed from Ensinger’s allowance of about 1 hour per 10 mm of cross-section at about 120 °C (248 °F)
Cross-section, mm (in) Approximate heating time, hours
20 (0.8) 2
40 (1.6) 4
60 (2.4) 6
80 (3.1) 8
100 (3.9) 10

The table is an allowance for planning, not a validated cycle. Ensinger frames the warm drilling itself as a measure for extreme cases, and the cool-down before finishing adds time that the table does not show.

Reading a Failed Hole

MCAM’s troubleshooting chart for drilling lists ten faults: a tapered hole, a burned or melted surface, chipping, chatter, feed marks or spiral lines on the bore, oversize holes, undersize holes, holes that are not concentric, a burr at cut-off, and fast dulling of the drill. The causes it names repeat across the columns: a drill sharpened incorrectly or off-center, a web that is too thick, too little or too much clearance, a feed that is too heavy or too light, too much rake, a point angle that is too great or too small, and a drill that does not pass completely through the piece.

The pattern is useful because it points back to three settings. Most hole faults in the chart come from the drill grind, the feed, or the support of the part. Cutting speed appears less often, which matches the makers’ general advice that plastic tolerates high speeds but not rubbing.

Röhm adds a check that costs nothing. Start the hole with a slow feed until all cutting edges have engaged, increase the feed for the body of the hole, and slow down again just before the drill exits. Thin sheet should lie on a flat, solid support so the exit side does not chip. Tangram’s list makes the same point about breakthrough: chipping at exit is a separate failure from heat inside the hole, and it is fixed by feed control at the end of the stroke.

Signs a Deep Hole Is Running Hot

  • A chip that turns from a continuous ribbon to a molten string partway down the hole.
  • Discoloration or a glazed, smeared wall when the drill is withdrawn.
  • A drill that grabs or squeals as the flutes pack.
  • A part that is warm to the touch around the hole after a single pass.

Any of these is a signal to shorten the peck, check the drill edge, or add air or coolant before the next part.

Tapped Holes and Pilot Drill Size

A deep hole that will be tapped adds one more variable. MCAM tells machinists to check the actual cutting size of the pilot drill, because most plastics close up after drilling and the smaller hole can make taps tight. The nominal tap-drill size from a metal chart is only a starting point. Ensinger quantifies the margin it uses: taps often need an allowance of about 0.1 mm (0.004 in), depending on the material and the diameter.

Thread cutting is the second exception in Ensinger’s list of operations that need coolant. Its preferred tools are chasing tools for male threads and thread milling for female threads, and it advises against dies. MCAM recommends spiral taps over straight ones, rigid tapping cycles on CNC machines where possible, and good-quality taps.

Inserts are a design decision rather than a drilling one. MCAM says threaded inserts are not needed in most of its engineering materials, but recommends them where a joint sees strong vibration or repeated assembly. Where self-tapping inserts are used, it asks for a check that the hole has not closed after insertion.

What to Put on the Drawing and the Purchase Order

A buyer cannot set the peck interval, but the drawing and the order can prevent the failures that come from missing information. The following notes take a line each and remove guesswork from the shop.

  • The depth and diameter of each hole, so any hole deeper than two diameters is visible at quoting.
  • Whether the hole may be drilled from both ends or only from one side.
  • The exact grade and stock form, because a reinforced grade changes the drill, the speed and possibly the pre-warming.
  • Any coolant restriction for the grade, such as dry machining only for a flame-retardant UHMW-PE.
  • Whether a large bore may be produced by staged drilling and boring.
  • The measurement condition for bore diameters: after the part has cooled to room temperature.
  • For tapped holes, the thread class and whether inserts are acceptable.

The drawing does not tell the shop how to drill, but it can tell the shop which hole is deep, which grade is in the bar and when the bore is measured. Those three facts decide most deep-hole outcomes.

For deep bores in nylon, acetal or PEEK across a run of tens or hundreds of parts, low-volume plastic CNC with bridge production behind it keeps the same drill grind, peck interval and cool-down from the first article through the last batch.

Sources and Further Reading

Request a Plastic CNC Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Plastic CNC chosen.

Request a Quote