GradeAnnealingAcrylic

Thermal Expansion of Machined Plastic Parts by Material and Size

Every machined plastic dimension has a temperature, and the material decides how many degrees of drift a given tolerance can absorb.

Four long CNC machined bars in white acetal, white UHMW polyethylene, amber PEI and black acetal, each with a precise bore at both ends.

A 1 m (39.4 in) sheet of cast acrylic grows 1.4 mm (0.055 in) when it warms by 20 K, and Röhm prints that sum in its machining guide for PLEXIGLAS. Shrink the sheet to a 100 mm (3.94 in) machined block and the same 20 K moves it by 0.14 mm, which is larger than the best tolerances Mitsubishi publishes for a 100 mm feature in acetal or nylon (0.09 mm) and in PEI (0.06 mm). Plastics grow with temperature far more than the metals most drawings were written for, and machined parts are measured in rooms that are never the temperature the drawing assumes.

The sections below put numbers on that growth for the materials in these resources, from the coefficients on their data sheets, and then set the numbers beside the tolerance a buyer writes. Every coefficient is a published figure and every growth value is arithmetic on it.

Thermal Expansion of Machined Plastic Parts per 10 Degrees

The coefficient of linear thermal expansion, CTE, is the fractional length change per degree. Plastic sheets print it in 10⁻⁶ per kelvin or in inches per inch per degree Fahrenheit, and the two convert by a factor of 1.8: one in/in/°F is 1.8 per °C. Table 1 collects values from the sheets used in these resources and multiplies them out for three lengths and a 10 K change.

Table 1. Linear thermal expansion from published sheets, and growth over 10 K (18 °F) for 25, 100 and 200 mm
Material and source CTE, per K (per °F) 25 mm (0.98 in), mm (in) 100 mm (3.94 in), mm (in) 200 mm (7.87 in), mm (in)
UHMW-PE, TIVAR 1000 Virgin, Mitsubishi 200 x 10⁻⁶ (11 x 10⁻⁵) 0.050 (0.0020) 0.200 (0.0079) 0.400 (0.0157)
Acetal homopolymer, TECAFORM AD (Delrin 150 series), Ensinger 122 x 10⁻⁶ (6.8 x 10⁻⁵) 0.031 (0.0012) 0.122 (0.0048) 0.245 (0.0096)
HDPE, Spartech SP-1010 108 x 10⁻⁶ (6.0 x 10⁻⁵) 0.027 (0.0011) 0.108 (0.0043) 0.216 (0.0085)
Cast acrylic, PLEXIGLAS GS, Röhm 70 x 10⁻⁶ 0.018 (0.0007) 0.070 (0.0028) 0.140 (0.0055)
PEI, unfilled, TECAPEI natural, Ensinger 56 x 10⁻⁶ (3.1 x 10⁻⁵) 0.014 (0.0006) 0.056 (0.0022) 0.112 (0.0044)
PEI, 30 % glass, TECAPEI GF30, Ensinger 20 x 10⁻⁶ (1.1 x 10⁻⁵) 0.005 (0.0002) 0.020 (0.0008) 0.040 (0.0016)
Steel, for comparison, NIST about 12 x 10⁻⁶ 0.003 (0.0001) 0.012 (0.0005) 0.024 (0.0009)

The order is the point. UHMW-PE moves 16 times as far as steel, acetal homopolymer 10 times, HDPE 9 times, unfilled PEI almost 5 times, and glass-filled PEI under 2 times. Mitsubishi’s machining guide gives the general version, that thermal expansion of plastics is up to 10 times higher than that of metals, and the table shows UHMW-PE exceeding even that against steel.

The steel value comes from a NIST paper on the history of the 20 °C reference temperature, which gives the CTE of steel as about 12 x 10⁻⁶ per °C and brass as about 24 x 10⁻⁶. It is a round number for comparison, not a grade.

A 100 mm feature in acetal grows about 0.12 mm for each 10 K, and the same feature in glass-filled PEI grows about 0.02 mm. The material choice sets the size of the swing before any tolerance is written.

What ASTM D696 and E831 Measured for These Coefficients

Most of the sheets cite ASTM D696 for the coefficient. Its scope covers the determination of the coefficient of linear thermal expansion for plastics with a coefficient greater than 1 µm/(m·°C), using a vitreous silica dilatometer, and the title restricts it to temperatures between −30 °C and 30 °C. The standard says another test method, E228, is to be used outside that range. On astm.org the 2016 edition shows as historical and a 2024 edition as active.

Three statements in the standard shape what a number means:

  • The material has to show negligible creep or elastic strain under the stresses imposed, insofar as these affect accuracy.
  • Thermal expansion of a plastic has a reversible component with superimposed changes in length due to moisture content, curing, loss of plasticizer or solvents, release of stresses and phase changes. The method is intended to exclude those factors as far as possible, and the standard admits it cannot exclude them completely.
  • For that reason the method gives only an approximation to the true thermal expansion.

An alternative is ASTM E831, thermomechanical analysis, which measures over a scanned range from −120 °C to 900 °C and recommends a lower limit of 5 µm/(m·°C). D696 itself notes there is no known ISO equivalent to the standard. The sheets in Table 1 use both: Ensinger cites E831 for its unfilled PEI and D696 for the glass-filled grade, and Mitsubishi cites E831 for TIVAR 1000.

Two limits follow for a buyer. The coefficient on a D696 sheet is a value near room temperature, from −30 °C to 30 °C, and a part that runs at 80 °C or 150 °C lies outside the range the standard covers. The range a figure belongs to changes it as well: Mitsubishi prints TIVAR 1000 at 110 µin/in/°F over −40 to 150 °C (−40 to 300 °F) by E831, which is 198 x 10⁻⁶ per K, and at 200 µm/(m·K) over 23 to 100 °C, two figures for one bar that differ because they span different temperatures.

The 20 °C Reference and the 23 °C Data Sheet

A dimension has a temperature. The NIST paper states the principle in its abstract: a part dimension changes with temperature because of thermal expansion, and since 1931 industrial lengths have been defined as the size at 20 °C. Adoption of 20 °C by the International Committee for Weights and Measures was unanimous, on 15 April 1931.

The data sheets use a different temperature. Mitsubishi’s sheet states that all its tests are done at room temperature, 23 °C (73 °F), and Ensinger’s tables print their values at 73 °F. A drawing that cites a property from a sheet and a dimension from the metrology convention is quoting two temperatures 3 K apart.

Over 3 K a 100 mm feature changes by 0.059 mm (0.0023 in) in UHMW-PE, 0.037 mm (0.0014 in) in acetal homopolymer, 0.032 mm (0.0013 in) in HDPE, 0.021 mm (0.0008 in) in cast acrylic, 0.017 mm (0.0007 in) in unfilled PEI and 0.006 mm (0.0002 in) in glass-filled PEI.

For a feature toleranced at ±0.1 mm (±0.004 in), that is a small share and no cause for concern. Toleranced at ±0.05 mm (±0.002 in) in UHMW-PE, it it is more than half the band. A drawing that does not say whether the part is measured at 20 °C or 23 °C gives the supplier and the buyer room to disagree by the whole difference.

How Much Temperature Moves a 100 mm Feature by 0.05 mm

The growth per kelvin turns into a more useful figure when it is run backward. Table 2 divides a 0.05 mm band by the growth per kelvin and gives the temperature change that uses it up.

Table 2. Temperature change that moves a 100 mm (3.94 in) feature by 0.05 mm (0.002 in), from the CTE values in Table 1
Material Growth per K over 100 mm Temperature change that uses up 0.05 mm
UHMW-PE 0.0200 mm (0.00079 in) 2.5 K (4.5 °F)
Acetal homopolymer 0.0122 mm (0.00048 in) 4.1 K (7.4 °F)
HDPE 0.0108 mm (0.00043 in) 4.6 K (8.3 °F)
Cast acrylic 0.0070 mm (0.00028 in) 7.1 K (12.8 °F)
Unfilled PEI 0.0056 mm (0.00022 in) 9.0 K (16.2 °F)
Glass-filled PEI, 30 % 0.0020 mm (0.00008 in) 25 K (45 °F)
Steel 0.0012 mm (0.00005 in) 42 K (75 °F)

A tolerance of 0.05 mm on a 100 mm acetal feature is held by a part that stays within about 4 K of the measurement temperature. Bench temperature 3 K above 20 °C already takes up most of it. The same band on a glass-filled PEI part tolerates a 25 K swing.

A worked case puts the table next to a published tolerance. Mitsubishi’s guide lists a best tolerance of 0.09 mm for PA, POM and 207 PTFE at 100 mm, 0.06 mm for the group that holds PEI, and 0.15 mm for HDPE. A workshop that drifts by 6 K between morning and afternoon, say from 20 to 26 °C, moves a 100 mm acetal feature by 0.073 mm, which is 81 percent of the 0.09 mm figure.

The same 6 K moves an HDPE feature by 0.065 mm, 43 percent of 0.15 mm, and an unfilled PEI feature by 0.034 mm, 56 percent of 0.06 mm. Mitsubishi does not say whether its figures are a plus-and-minus value or a total band, so the shares are rough. They still show that for acetal the room’s temperature is already most of the published tolerance.

A band of 0.05 mm on a 100 mm acetal feature is used up by about 4 K, and the same band on a glass-filled PEI feature by about 25 K.

None of this says the tolerance is unachievable. It says the temperature is part of the tolerance, and that the same line on the drawing means very different things for two materials.

Moisture, Stress and Machining Heat Add to the Growth

Expansion with temperature is the term that can be calculated. Others are added to it, and the sources name them.

Röhm’s guide says acrylic has a high coefficient of linear thermal expansion and that moisture also has an influence on dimensional stability, though less than heat. It adds that mechanically treating only one sheet surface can distort the workpiece slightly, that the distortion can be reversed by annealing, and that annealing before machining avoids it in more complex technical parts. The ASTM D696 scope names the same list of non-thermal contributions: moisture content, release of stresses and changes in phase.

Mitsubishi’s turning tips add the machining term. The guide advises roughing out large sections and leaving them for 24 hours, and notes that most diameters will grow, so the lowest dimension should be aimed at when setting the tool. Tangram’s guide, for its part, says heat builds up faster in the cutting zone and that parts can move after machining through stress relaxation.

Röhm’s annealing conditions for acrylic show how slowly stress leaves a part. For PLEXIGLAS GS the temperature is 80 °C, or up to 100 °C for unformed parts, and the annealing time in hours is the thickness in millimeters divided by 3, with a minimum of 2 hours. Cooling in the oven takes the thickness in millimeters divided by 4 hours, at no more than 15 °C per hour, and the part leaves the oven no warmer than 60 °C. A 12 mm acrylic block is therefore in the oven 4 hours and cooling for 3, and a measurement taken before that has run reads a part still carrying its stress.

Three effects can overlap on a freshly cut part:

  • Heat from the cut leaves the part warm, so the first measurement reads large.
  • Stress released by material removal shifts the part over hours.
  • Moisture alters the size over days to weeks, at a rate the sheets print as a percentage of mass and not as a length.

A first-article measurement taken at the machine, warm and fresh, is not the size the part keeps. One taken after rest at the stated temperature is.

Plastic Parts in Metal Housings and Metal Pins

The ratio of roughly 5 to 16 times matters most where a plastic part meets a metal one. NIST’s own example describes the difficulty: two mating parts of different materials, assembled at one temperature and used at another, grow by their coefficients times the temperature difference, and the part with the larger coefficient may no longer assemble or fit.

Take a 50 mm (1.97 in) acetal homopolymer bushing pressed into a steel bore, then warmed by 30 K from 20 to 50 °C. By the Table 1 coefficients the bushing diameter grows by 122 x 10⁻⁶ x 50 mm x 30 K, or 0.18 mm (0.007 in), and the steel bore by 12 x 10⁻⁶ x 50 mm x 30 K, or 0.018 mm (0.0007 in). The fit has tightened by about 0.165 mm in diameter. Warming a bushing that starts as a clearance fit eats into the clearance at the same rate, and cooling reverses both.

Glass-filled PEI changes the picture. Its 20 x 10⁻⁶ per K is only 1.7 times the 12 x 10⁻⁶ NIST gives for steel, so the same 50 mm bushing warmed by 30 K grows 0.030 mm against 0.018 mm for the steel bore, a difference of 0.012 mm instead of 0.165 mm.

The numbers are idealized, since a pressed bushing is constrained and the plastic does not expand freely. They still show why a plastic part in a metal housing is toleranced with both materials’ coefficients in view, and why the sheets for glass-filled grades, with coefficients nearer steel, are the ones to look at when a fit has to hold across a temperature range.

What to Write on the Drawing and the Order

The drawing is where the temperature is fixed. A short set of lines turns a tolerance on a plastic part into one that two parties can check.

  • State the measurement temperature, 20 °C (68 °F) under the metrology convention or 23 °C (73 °F) to match the data sheets, and use one on every feature.
  • Give a rest time after machining and before inspection, so heat and early stress release are out of the reading.
  • Name the grade, with filler and percentage, since the coefficient changes by a factor of nearly three between unfilled and 30 percent glass-filled PEI.
  • For fits to metal, give the service temperature range and say which side of the fit is allowed to move.
  • Read the CTE on a sheet as typical, from a test between −30 and 30 °C, and ask the supplier for the grade’s own value when the part runs outside that range.
Table 3. Three temperatures that appear on one plastic part
Temperature Where it comes from What it governs
20 °C (68 °F) industrial length reference since 1931 (NIST) the size a dimension is defined at
23 °C (73 °F) conditions stated on data sheets (Mitsubishi, Ensinger) the temperature of the property values
service temperature the application the size the part has in use

A drawing note that carries all of this reads like this: dimensions at 20 °C after 24 hours at that temperature; coefficient of the named grade as published by its maker; fit between bushing and housing checked at both ends of a 20 to 50 °C service range. Each clause removes one disagreement that otherwise shows up at inspection, when a part that left the machine warm measures differently on the bench.

For one to a few hundred plastic parts where fit across a temperature range decides the design, low-volume plastic CNC followed by bridge production is the stage to measure the first articles at the stated temperature and confirm the fit before a tool is cut.

Sources and Further Reading

Request a Plastic CNC Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Plastic CNC chosen.