A hole drilled in acetal can read under its drill’s diameter because the plastic closes in behind the cutting edge. Mitsubishi’s guide to machining plastic parts states it in one line: most plastics close up after drilling, which can make taps tight. Tangram Technology’s guide names the same fault for POM in its table, listing undersized holes unless an adequate cut is provided.

The sections below put published numbers on the hole, from the cutting data to the tolerance tables, and name the faults that move a hole’s size in each direction.

Why Holes in Plastic Come Out Undersize and What Else Moves Them

A hole in plastic differs from one in metal in four ways, and each has a published source.

Heat builds fastest in a drill. Tangram calls drilling the most problematic machining operation for plastics because it combines concentrated heat with chip congestion in a confined space, and lists smearing, local melting, internal stress, cracking and dimensional error as the results. Mitsubishi adds that heat builds up especially when hole depth is greater than twice the diameter.

The material springs. Plastics are much more elastic than metals, the Mitsubishi summary states, and elastic relaxation of the hole wall after the drill leaves is the natural reading of the closing-up the guide describes.

The hole carries stress. Mitsubishi notes that machining can leave residual stresses, and Röhm’s guide on acrylic lists drilling and screw fastening among the causes of tensile stress that annealing relieves.

The drill itself has a size, and its geometry changes the hole. Mitsubishi’s troubleshooting table ties oversize holes to a drill ground off-center, a web that is too thick, insufficient clearance, a feed that is too heavy and a point angle that is too great, and undersize holes to a dull drill, too much clearance and a point angle that is too small.

A drilled hole in plastic can end up under size from elastic closing, over size from a badly ground drill, and out of round or tapered from heat. The tolerance depends on which of these the process controls.

Published Hole and Feature Tolerances by Diameter

Mitsubishi’s guide prints a table of best tolerances by size, in millimeters, for five groups of materials, with a note that extra-precise tolerances can require special tooling and challenging machining steps. The table lists size, not feature type, so for a hole the size is its diameter. Nothing in the guide says whether the figures are a total band or a plus-and-minus value, and the tolerance shown is its own capability, not a general standard.

Table 1. Published best tolerance by size, Mitsubishi guide to machining plastic parts, selected sizes, mm (in)
Size, mm (in) HDPE PEI, PC, PEEK, PPS, PET-P group PA, POM, 207 PTFE PEEK with fillers PAI, PBI
5 (0.20) 0.05 (0.0020) 0.02 (0.0008) 0.02 (0.0008) 0.02 (0.0008) 0.02 (0.0008)
10 (0.39) 0.05 (0.0020) 0.02 (0.0008) 0.03 (0.0012) 0.02 (0.0008) 0.02 (0.0008)
25 (0.98) 0.05 (0.0020) 0.03 (0.0012) 0.04 (0.0016) 0.03 (0.0012) 0.03 (0.0012)
50 (1.97) 0.08 (0.0031) 0.04 (0.0016) 0.05 (0.0020) 0.03 (0.0012) 0.03 (0.0012)
100 (3.94) 0.15 (0.0059) 0.06 (0.0024) 0.09 (0.0035) 0.05 (0.0020) 0.04 (0.0016)

The first thing the table shows is that tolerance widens with size. HDPE holds 0.05 mm up to 25 mm and 0.15 mm at 100 mm. The PEI group goes from 0.02 mm at 5 mm to 0.06 mm at 100 mm.

The second is that material groups separate. At 25 mm the PEI and PEEK group holds 0.03 mm, and the PA, POM and PTFE 207 group holds 0.04 mm. Out at 100 mm the second group loosens to 0.09 mm against 0.06 mm.

No reason for the grouping is given. Sheets for the materials involved suggest one: Ensinger prints an expansion coefficient of 122 x 10⁻⁶ per K for its acetal homopolymer stock and 56 x 10⁻⁶ per K for its unfilled PEI, so the same temperature drift moves the acetal hole more than twice as far.

Third, the guide’s table is a capability of one shop group under its own process. A buyer should read it as a statement that holes of 5 to 25 mm in these materials can be held to a few hundredths of a millimeter, and ask a supplier for its own figures on the grade and size at hand.

Drilling Data That Keep the Hole Round

The same guide publishes drilling data by material group, and Tangram prints speeds and feeds for the common plastics. Table 2 sets the two together for four materials.

Table 2. Drilling starting values from Mitsubishi’s guide and Tangram Technology’s guide
Material Cutting speed Vc Feed Tool and geometry
POM and PA (Mitsubishi) 50 to 100 m/min (165 to 330 ft/min) 0.1 to 0.3 mm/rev (0.004 to 0.012 in/rev) HSS or carbide, point angle 90 to 120°, relief 5 to 10°, rake 3 to 5°
UHMW-PE (Mitsubishi) 50 to 100 m/min (165 to 330 ft/min) 0.1 to 0.3 mm/rev (0.004 to 0.012 in/rev) HSS or carbide, same geometry
PEI and PC (Mitsubishi) 50 to 100 m/min (165 to 330 ft/min) 0.1 to 0.3 mm/rev (0.004 to 0.012 in/rev) carbide, same geometry
Glass- or carbon-filled PEI, PEEK (Mitsubishi) 50 to 80 m/min (165 to 262 ft/min) 0.1 to 0.3 mm/rev (0.004 to 0.012 in/rev) carbide or PCD/CVD diamond
PMMA (Tangram) 20 to 60 m/min (65 to 197 ft/min) 0.1 to 0.5 mm/rev (0.004 to 0.020 in/rev) acrylic softens when heated, light cuts

Spindle speed follows from the cutting speed and the drill diameter. Tangram prints the formula: spindle speed in rev/min is 1,000 times the cutting speed in m/min divided by the product of pi and the diameter in millimeters. For the 50 to 100 m/min range that gives, for a 6 mm drill, 2,650 to 5,300 rev/min, for a 12 mm drill 1,330 to 2,650 rev/min, and for a 25 mm drill 640 to 1,270 rev/min.

Röhm’s guide gives a data point to test the formula against. For acrylic drilled with a 25 mm drill at a feed of 0.1 to 0.3 mm/rev, its most favorable speed is 510 rev/min, which by the formula is a cutting speed of about 40 m/min, inside the 20 to 60 m/min Tangram prints for PMMA. The two guides agree.

Röhm’s guide shows what the numbers prevent, using a set of three drilled holes in PLEXIGLAS GS. When speed or feed is too high, the chip is crumbly and the cut uneven. A speed or feed that is too slow overheats the hole, which shows signs of decomposition and a molten chip.

At the right speed and feed, the wall is smooth and the chip flows continuously. Tangram makes the same point in general terms, that slow and gentle is not automatically safer, because an overly light cut rubs and rubbing makes heat. A hole in the overheated state is also a hole whose size has drifted before it is measured.

Treat the speeds as starting points. Tangram calls its own table indicative, and Mitsubishi’s summary tells the machinist to experiment with fixtures, tool materials, angles, speeds and feeds to obtain optimum results.

The rules around those numbers are consistent across the sources.

  • Peck. Mitsubishi says frequent pull-outs are necessary on small holes, and Tangram recommends peck drilling for chip removal.
  • Use a slow spiral drill on small holes. The guide says a low helix drill allows better swarf removal on holes of 0.5 to 25 mm.
  • Thin the web of larger drills. For holes of 25 mm and larger the guide advises a thinned web to reduce friction and heat.
  • Relieve the drill. Tangram recommends relief grinding to reduce rubbing, and extra care at breakthrough to avoid chipping on exit.
  • Cool the deep hole. Mitsubishi recommends a cooling liquid when depth exceeds twice the diameter, with nonaromatic water-soluble coolants for amorphous plastics.

What the Troubleshooting Table Says About Hole Size

Mitsubishi’s table of drilling faults reads as a list of ways a hole misses its size, and Table 3 lists the ones that change dimension.

Table 3. Drilling faults that move hole size or shape, causes as listed in Mitsubishi’s guide
Fault Causes listed
Oversize hole drill ground off-center, web too thick, insufficient clearance, feed too heavy, point angle too great
Undersize hole dull drill, too much clearance, point angle too small
Tapered hole incorrectly sharpened drill, insufficient clearance, feed too heavy
Hole not concentric feed too heavy, spindle speed too slow, drill-off leaves a nib that deflects the drill, web too thick, drill speed too heavy at the start, drill not mounted on center, drill not sharpened correctly
Burned or melted surface wrong type of drill, incorrectly sharpened drill, feed too light, web too thick
Feed marks or spiral lines feed too heavy, drill not centered, drill ground off-center

The causes cross over. A feed that is too heavy shows in four of six rows, and a feed that is too light burns the wall in the fifth. Insufficient clearance gives an oversize or tapered hole, while too much clearance gives an undersize one. The drill’s geometry decides the hole more than any single setting.

For a buyer, the practical reading is that a hole’s size is a property of the tool’s condition at that hole, and how often a supplier changes drills is a fair question.

Large Holes by Staged Drilling and Boring

Past about 25 mm, drilling alone becomes the wrong tool. Mitsubishi advises drilling large holes stepwise, and gives an example: a bore of 50 mm is made by drilling successively with 12 mm and 25 mm drills and then expanding the hole with a single boring tool. The guide also recommends thinned-web drills for holes from 25 mm up.

Tangram agrees from the other side. Its list of the best results includes staged opening of large holes and boring rather than drilling for larger or more sensitive material.

The sequence has a tolerance logic. Drills open the hole in steps that keep heat and chip load low, and the single boring tool takes the final size. Table values for 50 mm, 0.03 to 0.08 mm across the five groups, are published for the size and not for a stage, so a buyer should ask which stage a supplier’s figure belongs to.

Thin-walled work needs its own support. The guide suggests that for tubes one end can be bored and a blank put in to support the clamp force of the jaws, and Tangram advises supporting thin-walled tubes with internal plugs against chatter, deflection and out-of-round conditions. A bore cut in an unsupported thin wall is round only while the chuck is closed.

For a bore that needs the tightest figure, the guide’s turning tips apply. Rough out, leave the part for 24 hours, aim at the low end of the dimension because most diameters grow, and finish with a light cut after the part has settled.

Acrylic and Other Amorphous Plastics

Cast and extruded acrylic hold their holes differently because the drill has to scrape, not cut. Röhm’s guide states that twist drills for metal cannot be used on PLEXIGLAS unless the point angle is reduced from the normal 120° to between 60 and 90°, with a rake angle ground down to between 4 and 0°, and a clearance angle of at least 3°. The reason given is to avoid chipping at the exit side of the hole.

Two further rules from the same guide protect the hole. Holes should be slightly chamfered or countersunk to rule out notch effects altogether, and from a material thickness of 5 mm onwards a cooling lubricant, a drilling emulsion compatible with acrylic, is advised. Drilled under those conditions at 0.1 to 0.3 mm/rev, the guide says holes have nearly transparent, silky matte walls, and that reamers of the kind used in metalworking improve the surface further.

Mitsubishi’s cooling notes carry the same warning for the whole amorphous group, covering PC, PPSU, PEI and PSU. Mineral-oil-based cutting fluids may contribute to stress cracking, and parts cut with coolant should be washed in isopropyl alcohol and pure water right away.

Drilling and tapping depend on the same fact: most plastics close up after the drill, so the pilot size is the one to measure on the real grade.

Threaded Holes and Inserts

A drilled hole is the first step of a tapped one, and the closing-up behavior matters most there. Mitsubishi’s tips give four rules for tapping and turning threads: use spiral taps, not straight ones, use rigid tap cycles on CNC machines where possible, check the pilot drill size, and use high-quality taps. The guide states that for pilot holes for internal threads, the actual cutting size of the drill should be checked, because most plastics close up and can make the tap tight.

Inserts change the answer. The guide says threaded inserts are not required when machining most of its engineering materials, but are recommended where there are strong vibrations or repeated clamping and unclamping. Self-tapping inserts are the most popular, with cautions: pre-tap slotted inserts, check that there is no closure after insertion, and consider inserts with a cross hole to cut.

The tolerance that matters for a threaded hole is the pilot diameter, and the number comes from checking the drill’s actual cutting size on the material and the grade in hand.

The edge of the hole needs the same attention as the wall. Mitsubishi lists deburring tools for plastics, sharp knives or rotating hooks, and says tool sharpness is what decides the result, while countersink tools of the kind it shows do not cut too deep or chatter. Hard plastics can be lightly abraded wet and dry, and rotary stones work on some.

Röhm’s advice for acrylic is the same in spirit: chamfer or countersink the hole to rule out notch effects. A hole measured before its burr is removed reads small, and one deburred with a heavy tool reads large.

What to Write on a Hole Call-Out

A hole call-out on a plastic part is a request for a process and a measurement, and the sources suggest what it should carry.

  • The diameter, depth and any chamfer, with the chamfer stated for acrylic and amorphous grades.
  • Tolerance, and the stage it applies to: drilled, reamed or bored.
  • Measurement temperature and a rest time after machining, since the hole moves with heat and stress.
  • Coolant, and which one is allowed, for amorphous grades.
  • For tapped holes, the thread, the pilot size and whether an insert is wanted.

For one to a few hundred plastic parts with tight bores, low-volume plastic CNC followed by bridge production lets the first articles confirm the stage and the measurement before the pattern is repeated.

Sources and Further Reading

Request a Plastic CNC Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Plastic CNC chosen.

Request a Quote