BurrFirst ArticleResin

Acetal Homopolymer and Copolymer Stock for CNC Machined Parts

Homopolymer is stiffer and harder, copolymer is sold porosity-free with less water uptake and less thermal growth, and the stock a part is cut from decides which it inherits.

CNC machined acetal parts, white and black POM spur gears, flanged bushings and a small manifold block with drilled ports, smooth satin plastic with fine tool marks.

Ensinger, which extrudes both kinds of acetal into rod and plate, prints a linear thermal expansion of 6.8 x 10⁻⁵ in/in/°F for its homopolymer stock and 4.7 x 10⁻⁵ for its copolymer stock. On a 100 mm (3.94 in) feature and a 10 °C (18 °F) rise, that is 0.12 mm (0.0049 in) against 0.085 mm (0.0034 in). Two materials sold under one name, acetal, move by different amounts on the same drawing, and the difference is larger than many machined tolerances.

The pair is worth reading side by side before a part is quoted. The sections below take Ensinger’s published data for its two stocks, the standard that covers acetal shapes, the makers’ machining and annealing guidance, and the choices that follow for a machined part.

Acetal Homopolymer and Copolymer Differences in Machined Parts

Acetal, the polyoxymethylene or POM family, reaches a machine shop as two chemistries. Homopolymer chains repeat one unit; copolymer chains carry two. Homopolymer is POM-H, best known by the Delrin resin, and Ensinger makes its TECAFORM AD natural stock from white Delrin resin of the 150 series. Copolymer is POM-C, which Ensinger sells as TECAFORM AH natural and Mitsubishi as Acetron.

Ensinger states the difference in one sentence: in comparison to POM-C, POM-H has a slightly higher density, hardness and strength because of its higher crystallinity. Its feature lists then pull the pair apart by use. For the homopolymer it names good machinability, high stiffness, high fatigue strength, high creep resistance and very good abrasion resistance. For the copolymer it names porosity-free stock, low water absorption, good chemical resistance, easy machining and high dimensional stability.

Neither material is simply the better one. Homopolymer buys stiffness, hardness and short-term heat performance; copolymer buys cleaner stock, lower water uptake and less thermal growth, and the drawing decides which of those the part needs.

Homopolymer buys strength, stiffness and hardness. Copolymer buys porosity-free stock, lower water uptake and less growth with heat.

Acetal Stock Properties in Metric and Inch Units

Table 1 sets Ensinger’s two product pages side by side. Both publish inch-pound units with the ASTM method beside each value, so the metric values are conversions, rounded.

Table 1. Unfilled acetal stock shapes at 23 °C (73 °F), from Ensinger’s TECAFORM AD (POM-H) and TECAFORM AH (POM-C) pages, converted to metric
Property (test method) POM-H, TECAFORM AD natural POM-C, TECAFORM AH natural
Tensile strength at yield (ASTM D638), MPa (psi) 75.8 (11,000) 64.1 (9,300)
Tensile modulus (ASTM D638), GPa (psi) 2.41 (350,000) 2.28 (330,000)
Elongation at break (ASTM D638) 25 % 40 %
Flexural strength (ASTM D790), MPa (psi) 96.5 (14,000) 89.6 (13,000)
Flexural modulus (ASTM D790), GPa (psi) 3.24 (470,000) 2.76 (400,000)
Rockwell hardness (ASTM D785) M94 (R120) M86, R120
Heat deflection at 1.8 MPa (264 psi) (ASTM D648), °C (°F) 125 (257) 110 (230)
Heat deflection at 0.45 MPa (66 psi) (ASTM D648), °C (°F) 169 (336) 158 (316)
Melting temperature, °C (°F) 175 (347) 165 (329)
Linear thermal expansion (ASTM D696), per K 122 x 10⁻⁶ 85 x 10⁻⁶
Water absorption 24 h / saturation (ASTM D570), % 0.25 / 0.90 0.18 / 0.80
Wear factor K (ASTM D3702), 10⁻¹⁰ in³·min/(ft·lb·h) 55 65
Service temperature, long term / intermittent, °C (°F) 85 / 149 (185 / 300) 91 / 141 (195 / 285)
Flammability (UL 94) HB HB

Read across a row and the ranking holds in most of them. Homopolymer is stronger by about 12 MPa at yield, stiffer in flexure by about 17 percent, and deflects under load at a temperature 15 °C higher. Copolymer stretches further before it breaks, takes up less water and grows less with heat. The service temperatures run the other way from the deflection figures: copolymer carries the higher long-term rating, homopolymer the higher intermittent one.

The rows that do not move are as useful. Both stocks list a density of 1.41 g/cm³, a dynamic coefficient of friction near 0.2 and a UL 94 HB rating, so neither is a flame-rated material. Plan for the ranking in each row, not for the decimal.

Centerline Porosity in Acetal Rod and Plate

Extruded acetal can carry a seam of fine pores along the centerline of rod and plate, where the core of the section freezes last. It does not appear in a property table, yet it sits exactly where a machined manifold, a bushing bore or a thin web will one day be cut.

The standard for acetal shapes treats it as a property. ASTM D6100 lists porosity level among the properties it sets for POM sheet, plate, rod and tubular bar, beside tensile strength, elongation, modulus, dimensional stability and Izod impact. Ensinger sells its copolymer stock on the point, describing TECAFORM AH natural as an unfilled, porosity-free POM-C, and makes no such claim on the homopolymer page.

Where the machined part crosses the centerline, the seam matters. A few checks follow from where it sits:

  • A part that holds fluid or gas, such as a manifold block, a valve body or a seal carrier, comes from stock sold as porosity-free, or from a plate thin enough that its core is machined away.
  • Drilling a bore on the stock’s axis puts the drill straight down the line where pores would sit. Offsetting the bore, or choosing a stock size that cuts the part away from the centerline, keeps them out of the wall.
  • Webs machined from the middle of a thick plate keep the seam in the web, and the same web taken from nearer a face does not.
  • A pressure or leak test belongs on the first article of any fluid part, whichever chemistry was bought.

None of this appears on the drawing. It sits in the stock choice, and that choice is the buyer’s to make.

A porosity seam can run along the axis of acetal rod and plate. Fluid-holding parts and axial bores are where it shows, and stock sold as porosity-free is the lower-risk choice.

Stock Sizes and Tolerances Before the First Cut

The bar has a tolerance of its own before the cutter touches it. Ensinger’s stock tables list its acetal rod with a plus-only tolerance on diameter: plus 0.002 in (0.05 mm) and minus nothing up to 1 in (25.4 mm), plus 0.005 in (0.13 mm) up to 2 in (50.8 mm), and larger allowances above that. A rod is therefore never undersize, and a part that uses the stock diameter as a finished surface carries the bar’s tolerance, not the machine’s.

Ensinger’s catalog gives the range of shapes it makes in copolymer: rods from 3 to 300 mm (0.12 to 11.8 in) in diameter, plates from 0.5 to 150 mm (0.02 to 5.9 in) thick and tubes from 20 to 435 mm (0.8 to 17.1 in). Common sizes are made to stock in both chemistries, and a grade or size outside the program means a made-to-order bar.

ASTM D6100 adds the stock-shape side of the same point: its dimensional requirements cover thickness tolerance, length camber and width bow. A part machined from the full thickness of a plate inherits them, and the raw bar needs enough oversize to clean up.

Machining Acetal on a Mill and a Lathe

Acetal sits at the easy end of the plastics machining scale. Tangram Technology’s guide to machining plastics rates POM as excellent and lists the usual faults: burrs when the tool is dull, heat when the cut rubs, and undersized holes unless the cutter is given enough to bite. It recommends single or low-flute cutters with sharp edges and generous chip clearance.

The same guide gives indicative cutting data for the family, reproduced in Table 2 with the guide’s conditions.

Table 2. Indicative cutting data for POM, from Tangram Technology’s machining guide
Operation Cutting speed Vc Feed Note in the guide
Milling 200 to 400 m/min (655 to 1,310 ft/min) up to about 0.5 mm per tooth (0.020 in) single-flute mills reduce frictional heat and give chip space
Turning 200 to 500 m/min (655 to 1,640 ft/min) 0.05 to 0.5 mm/rev (0.002 to 0.020 in/rev) long stringy chips can wrap the tool and the part
Drilling 50 to 100 m/min (165 to 330 ft/min) 0.1 to 0.3 mm/rev (0.004 to 0.012 in/rev) peck, relieve the drill, take extra care at breakthrough

These are starting points, not a program. The guide itself calls them indicative, and the right numbers depend on the cutter, the machine and the grade.

The principle behind the table is the one to remember. Tangram writes that slow and gentle is not automatically safer, because a light cut rubs, and rubbing makes heat. A cutter that is sharp, loaded with a real chip and given room to throw it clear produces a cleaner wall than one pushed gently through the stock.

Tangram groups POM among the semicrystalline plastics that often produce stringy chips and burr heavily when soft or tough, yet it rates the machinability as excellent and ties the faults to dull edges, rubbing and too little cut at the hole. A shop that keeps cutters sharp and chip loads real gets the clean walls the datasheet implies, and a shop that does not gets burrs on both chemistries alike.

Ensinger lists exceptional machining characteristics among the homopolymer’s strengths and easy machining among the copolymer’s, and Mitsubishi’s guide places both acetals in the same rows of its sawing, drilling and turning tables. On the machine the two chemistries are close; the differences that matter come back at the measuring table.

Work holding needs the same care as cutting. Plastics deform under clamp pressure that a metal part would not notice, and Tangram advises supporting thin sections and tubes, and treating tolerance as a stability problem rather than only a cutting problem. A bore finished while the part is squeezed in a chuck will return to a different shape when the chuck opens.

Dimensional Stability and Stress Relief After Cutting

Acetal takes up little water, which is part of why it holds size. Ensinger lists 0.25 percent after 24 hours and 0.90 percent at saturation for the homopolymer, and 0.18 and 0.80 percent for the copolymer, both at 23 °C. The sheets give no dimensional change for those figures, but the ranking is the useful part.

Internal stress is the larger movement. Ensinger’s stock catalog states that its stock shapes are annealed after production to reduce the internal tension created in manufacture, and Mitsubishi’s guide warns that extrusion, molding and machining can all leave residual stresses that redistribute and warp a part when material is removed. Tangram lists parts moving after machining through stress relaxation among the common faults.

Where a part needs an anneal between roughing and finishing, Mitsubishi gives one cycle for both acetals: a heat-up of 10 to 20 °C (18 to 36 °F) per hour to a hold of 155 °C (311 °F), 10 minutes per millimeter of wall, and a cool-down of 5 to 10 °C (9 to 18 °F) per hour, in air, nitrogen or oil. It lists a lower hold, 140 °C (284 °F), for its PTFE-filled homopolymer.

The buyer’s levers are narrow:

  • Ask which stock the supplier runs, by maker and grade, and whether it is sold as stress-relieved.
  • Rough the part and let it rest before finishing when it has thin ribs, a deep pocket or a flat that has to stay flat.
  • Material removal stays symmetric about the mid-plane, so one face does not release more stress than the other.
  • Annealing is for the geometry that needs it. Tangram’s guide says to use annealing selectively and only where it adds value.

Temperature moves the part even when stress does not. With the expansion figures of Table 1, a 100 mm feature grows about 0.12 mm in homopolymer and 0.085 mm in copolymer for a 10 °C rise. That is larger than most plastic tolerances a drawing asks for, which is why the measurement temperature belongs on the drawing.

What ASTM D6100 Says About Acetal Shapes

Stock shapes have a standard of their own. ASTM D6100, Standard Specification for Extruded, Compression Molded and Injection Molded Polyoxymethylene Shapes (POM), covers requirements and test methods for the material, dimensions, workmanship and properties of POM sheet, plate, rod and tubular bar, excluding pipe and fittings. The astm.org page lists the 2011 edition as historical, last updated 21 May 2014.

What the standard sets for a shape is a short list. Its properties include tensile strength, elongation at break, tensile modulus, dimensional stability, flexural modulus, Izod impact and porosity level, and the shape also has to meet dimensional requirements for thickness tolerance, length camber and width bow. The specimen may be pure polyoxymethylene or filled, lubricated or reinforced with carbon fiber, graphite, glass, PTFE, silicone, molybdenum disulfide or minerals.

For the buyer, three consequences follow.

  • A callout of POM on a drawing leaves homopolymer, copolymer and every filled variant open. Naming the chemistry and the maker’s grade closes that gap.
  • A claim that a shape meets D6100 covers the shape; the resin carries a specification of its own.
  • Stock allowances include camber and bow. A part machined from the full thickness of a plate inherits them, and the raw bar needs enough oversize to clean up.

The standard’s tables are not reproduced here and were not opened; they sit behind the purchase. What the public page confirms is the scope, the property list and the dimensional categories above.

Choosing Homopolymer or Copolymer for a Part

The choice comes down to what the part does and how big it is. Table 3 pairs the usual part features with the chemistry the published data favor, and names the row of Table 1 or the statement behind each.

Table 3. Feature-by-feature choice between POM-H and POM-C stock
Part feature Leans toward Basis
Stiff, strong part under load POM-H higher yield strength and flexural modulus (Table 1)
Short exposure to heat under load POM-H higher deflection temperature (Table 1)
Long-term service near its limit POM-C higher long-term service rating (Table 1)
Tight tolerance across temperature POM-C lower thermal expansion (Table 1)
Damp service or tight size in humidity POM-C lower water absorption (Table 1)
Bore on the stock axis, or fluid held in the part POM-C, porosity-free stock Ensinger’s porosity-free claim; D6100 porosity level
Wear surface, abrasion POM-H lower wear factor and very good abrasion resistance (Ensinger)
Part that bends before it breaks POM-C higher elongation at break (Table 1)

The rows that favor homopolymer depend on strength, stiffness and short-term heat, and the rows that favor copolymer depend on water, temperature growth and stock quality. None of them is an absolute, and a part that needs both stiffness and a clean bore is a case for asking the stock maker which grade and size it would cut it from.

Parts of either chemistry that start as a few prototypes and grow into repeat lots fit low-volume plastic CNC work and then bridge production, with the stock grade, maker and measurement temperature fixed on the drawing from the first article.

Sources and Further Reading

Request a Plastic CNC Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Plastic CNC chosen.

Request a Quote