Machining Tolerances by Part Size for Engineering Plastics

Published plastic tolerances widen with feature size and split by polymer group, so a drawing has to state size, grade, temperature and rest.

CNC machined white acetal parts of three sizes, a small bushing, a mid-size flanged housing and a long flat bar with slots.

Between a 1 mm feature and a 200 mm one, the published machining tolerance for HDPE goes from 0.05 mm to 0.26 mm. The size grows 200 times and the tolerance grows five. That mismatch is the whole subject: a plastic part is held to a tolerance that depends on how large the feature is and on which polymer it is cut from, and a drawing that writes one general number for every feature of every material asks for something no supplier publishes.

Mitsubishi Chemical Advanced Materials is one of the few stock-shape makers that prints a table of its best machining tolerances by size and material group. This piece reads that table in millimeters and inches, shows what its numbers imply, and sets out what a buyer still has to say on the drawing for the numbers to mean anything.

Published Machining Tolerances by Feature Size and Material Group

Table 1 reproduces the Mitsubishi table for nine of its sizes, with inches beside each figure. The five groups are the guide’s own: HDPE; the group that holds PET-P, PC, PEEK, PTFE 500, PPS, PEI, PPSU and PSU; the group that holds PA, POM and PTFE 207; PEEK with fillers; and PAI with PBI.

Table 1. Best machining tolerance by size, Mitsubishi guide to machining plastic parts, mm (in)
Size, mm (in) HDPE PEI, PC, PEEK, PPS, PET-P group PA, POM, PTFE 207 PEEK with fillers PAI, PBI
1 (0.04) 0.05 (0.0020) 0.02 (0.0008) 0.02 (0.0008) 0.02 (0.0008) 0.02 (0.0008)
10 (0.39) 0.05 (0.0020) 0.02 (0.0008) 0.03 (0.0012) 0.02 (0.0008) 0.02 (0.0008)
20 (0.79) 0.05 (0.0020) 0.03 (0.0012) 0.03 (0.0012) 0.03 (0.0012) 0.02 (0.0008)
30 (1.18) 0.06 (0.0024) 0.03 (0.0012) 0.04 (0.0016) 0.03 (0.0012) 0.03 (0.0012)
50 (1.97) 0.08 (0.0031) 0.04 (0.0016) 0.05 (0.0020) 0.03 (0.0012) 0.03 (0.0012)
80 (3.15) 0.12 (0.0047) 0.05 (0.0020) 0.07 (0.0028) 0.04 (0.0016) 0.04 (0.0016)
100 (3.94) 0.15 (0.0059) 0.06 (0.0024) 0.09 (0.0035) 0.05 (0.0020) 0.04 (0.0016)
150 (5.91) 0.21 (0.0083) 0.08 (0.0031) 0.12 (0.0047) 0.06 (0.0024) 0.05 (0.0020)
200 (7.87) 0.26 (0.0102) 0.10 (0.0039) 0.15 (0.0059) 0.08 (0.0031) 0.07 (0.0028)

The guide’s full table has rows at 1 and 5 mm, then every 5 mm to 50 mm and every 10 mm to 200 mm, and the rows above are a selection. Above the table the guide carries a plain warning: these extra-precise tolerances can require special tooling and challenging machining steps.

Three limits on the table are worth stating before using it. The figures are headed “tolerances” in millimeters, and the guide does not say whether each is a total band or a plus-and-minus value. They are the maker’s best capability, labeled as such, and not a standard that a shop signs up to. The table also names a size and a material group, and does not name the feature, so a diameter, a length and a position are all read from the same line.

The chart above the table carries a sixth curve, labeled standard, that the table does not print as a column. It stays flat at 0.05 mm up to about 50 mm and climbs to about 0.15 mm near 150 mm. A buyer working from the numbers should use the table and treat the extra curve as context the guide does not explain.

The best published tolerance runs from 0.02 mm on a small feature in a stiff polymer to 0.26 mm on a 200 mm feature in HDPE. Material group moves it by a factor of two to four at the same size.

How Tolerance Widens With Size

Tolerance in the table is a nearly straight line against size, and its slope depends on the group. Between 100 and 200 mm, the HDPE figure rises by 0.11 mm, the PA and POM group by 0.06 mm, the PEI and PEEK group by 0.04 mm, and the filled PEEK and PAI groups by 0.03 mm. That is 1.1, 0.6, 0.4 and 0.3 micrometers of tolerance per millimeter of size.

Table 2. Tolerance as a share of size, from Table 1
Group At 10 mm At 100 mm At 200 mm
HDPE 0.50 % 0.15 % 0.13 %
PEI, PC, PEEK, PPS, PET-P group 0.20 % 0.06 % 0.05 %
PA, POM, PTFE 207 0.30 % 0.09 % 0.075 %
PEEK with fillers 0.20 % 0.05 % 0.04 %
PAI, PBI 0.20 % 0.04 % 0.035 %

A small feature is held to a larger share of its size than a large one. At 10 mm the PEI group’s 0.02 mm is 0.2 percent of the dimension, and at 200 mm its 0.10 mm is 0.05 percent. The floor of 0.02 mm at the small end looks like a property of the process, the tool, the setup and the measurement, more than of the polymer, since every group but HDPE shows the same 0.02 mm at 1 mm.

The share falls with size, and the width rises. For a buyer the useful reading is that a large plastic part gets a wider band in millimeters and a tighter one in relative terms. A drawing that gives 0.05 mm on every dimension from 5 to 200 mm is asking for 0.05 mm on a 200 mm acetal feature when the published best is 0.15 mm.

Why the Material Groups Separate

The guide does not explain its grouping. Data sheets suggest what sits behind it, and each suggestion has a number.

  • Expansion. At the same temperature drift, a polymer with a higher coefficient moves further. Ensinger gives its acetal homopolymer stock 6.8 x 10⁻⁵ in/in/°F (122 x 10⁻⁶ per K), its unfilled PEI 3.1 x 10⁻⁵ (56 x 10⁻⁶ per K) and its 30 percent glass PEI 1.1 x 10⁻⁵ (20 x 10⁻⁶ per K). That ratio of more than two to one is in the range of the spread between the acetal group and the PEI group at 100 mm, 0.09 mm against 0.06 mm, though the table does not claim the link.
  • Stiffness. A stiffer polymer deflects less under the cutter and the clamp. Tensile modulus runs from about 1.3 GPa for Spartech’s HDPE sheet to 2.3 to 2.4 GPa for Ensinger’s acetals and about 3 GPa for its PEI, and HDPE is the group with the widest tolerance. Expansion alone does not explain that, since Spartech’s HDPE coefficient of 108 x 10⁻⁶ per K sits below the acetal homopolymer’s.
  • Fillers. Glass and carbon fibers raise stiffness and cut expansion. The guide lists PEEK with fillers as a tighter group than unfilled PEEK in the PEI group.
  • Stock stability. Ensinger’s catalog states that its stock shapes are annealed after production to reduce internal tension, and Mitsubishi’s guide treats a further anneal as an option for tight-tolerance parts.

Tangram’s guide draws the same conclusion in one line of its summary: treat tolerances as a stability problem, not just a cutting problem. The table is a map of stability by polymer.

Reading the Table for Three Parts

Three examples show how the lines are read. Each uses only the published best, and each leaves out what a drawing adds on top.

An acetal boss 25 mm (0.98 in) across sits at the PA and POM column, where the best is 0.04 mm (0.0016 in). A tolerance of 0.05 mm is looser than that best by a small margin, and a tolerance of 0.03 mm is tighter than anything the guide prints for that size and group.

A PEI insulator 80 mm (3.15 in) long sits in the group with PC and PEEK, where the best is 0.05 mm (0.0020 in). With a thermal coefficient of 56 x 10⁻⁶ per K, a 5 K change moves it 0.022 mm, about 45 percent of that band.

An HDPE guide rail 150 mm (5.91 in) long sits in the widest column, with a best of 0.21 mm (0.0083 in). A drawing that calls a 0.1 mm band on such a rail asks for about half of the 0.21 mm the guide lists, a different request from the general tolerance a metal part of the same length would carry. Because the guide does not state its convention, the supplier’s answer to that call-out should say which band it is quoting.

In each case the useful move is the same: set the tolerance at or just outside the published best for the size and group, spend the tight tolerance on the one feature that carries the function, and leave the rest at the width the material can hold in the room it is measured in.

Spend the tight tolerance on the one feature that carries the function, and leave the rest at the width the material can hold in the room it is measured in.

A capability study turns that advice into a number. The method is general: machine a set of parts on the grade and geometry in question, measure each at a stated temperature after a stated rest, and compare the spread of results with the tolerance asked. Mitsubishi’s guide advises such studies on a shop’s own machines because the published table is a best case. A supplier that can show a spread for the polymer and the size on the drawing has answered the tolerance question with evidence, and one that quotes the table has answered it with a hope.

The table also leaves materials out. UHMW-PE, polypropylene and acrylic have no column, and HDPE is the only polyolefin listed. Mitsubishi’s own TIVAR 1000 sheet gives UHMW-PE an expansion of 200 x 10⁻⁶ per K, nearly double the 108 x 10⁻⁶ of Spartech’s HDPE, so a reasonable reader would not expect it to hold a tighter band than the HDPE column, though the guide does not say so. The guide is also metric only, and the inch figures in Table 1 are conversions made for this piece.

Features the Size Table Does Not Cover

Size is one tolerance, and the others are named by the same guide in its general rules.

Flatness and bow come from stress and from the extrusion centerline. Mitsubishi’s rules are to consider rod as well as plate, to machine equally to the centerline, and to cut pockets in intermediate steps. Its example shows a plate machined on one side only, which bows top and bottom about the centerline of the extrusion. The recommended solutions include starting with the thickest plate and moving the extrusion line away from machined features, machining slots in the opposite face, and balanced machining on both sides.

Mitsubishi’s guide adds the path to flatness on a part with a tight flat and an uneven contour: rough the part, anneal or rest it, and finish with a light cut, and remove material equally on both sides of the stock’s centerline, so that one face does not release more stress than the other.

Stock itself has tolerances. ASTM D6100 for acetal shapes lists thickness tolerance, length camber and width bow among the dimensional requirements, and EN 15860 for thermoplastic semi-finished products for machining lists, in its contents, tolerances for rods (diameter, length, roundness, straightness), hollow bars (including concentricity) and sheets (thickness, length and width, straightness), and a requirement on dimensional stability after heat treatment. The tables behind those clauses were not opened for this piece. What the contents show is that stock arrives with its own variation, and that a machined feature inherits some of it. A part that is later injection molded follows other rules again, with shrinkage and wall thickness setting the tolerance more than the cutter does, so the machined tolerance of a first lot is not a promise for the molded one.

How a Tolerance Is Checked and When

A tolerance in plastic has a time and a temperature as well as a size. The sources give four steps that matter.

  • Rest before measuring. Mitsubishi’s turning tips advise roughing out large sections and leaving them for 24 hours to improve tolerances.
  • Aim low. The same tips note that most diameters grow after cutting, so the lowest dimension is the target when setting the tool.
  • Measure at a stated temperature. The NIST paper on the 20 °C reference states that industrial lengths have been defined as the size at 20 °C since 1931, and the data sheets in these resources state 23 °C. A 100 mm acetal feature moves 0.037 mm between the two.
  • Study the machine. The guide advises capability studies on a shop’s own machines, which is a way of replacing the table’s best case with the shop’s actual spread on the polymer in hand.

Mitsubishi’s tips add two ways of keeping a part still while the cut is made: sliding head machines for small long sections, and, for tubes, boring one end and putting a blank in to support the clamp force of the jaws. Both bear on the 0.02 mm floor at the small end of the table.

The first article is where a buyer sees the answer. A first article measured at the stated temperature after the stated rest, on the real grade and geometry, is evidence, and the table is not.

What a Tolerance Call-Out on a Plastic Part Should Carry

A tolerance on a plastic part is the start of a conversation about a process. The call-out can end the conversation early by saying which features carry the function.

  • Tolerance only the features that need it. Mitsubishi warns that tight tolerances can require special tooling and challenging machining steps.
  • Tie each tolerance to a size and a material, and check it against the published best for that size and group.
  • Give the measurement temperature and the rest time.
  • Name the grade, with the filler and its percentage.
  • Note whether stress relief is wanted and at which stage.
Table 3. Tolerance requests and what each asks of the process
Request on the drawing What it asks of the process
0.02 mm on a 10 mm feature, acetal tighter than the published 0.03 mm best for that size and group
0.05 mm on a 10 mm feature, acetal looser than the published 0.03 mm best, with room for heat and rest
0.05 mm on a 100 mm feature, acetal tighter than the 0.09 mm published best
0.15 mm on a 100 mm feature, HDPE at the published best
0.05 mm on a 100 mm feature, glass-filled PEEK at the published 0.05 mm best
flatness on a plate with one-sided pockets stress relief or balanced cuts around the centerline

A request at or inside the published best is a request for evidence, and the useful reply is a measured spread on the grade, not a yes. Anything wider than the published best is a request the table already supports, and the saving in effort goes to the features that need it. Either way the call-out and the reply should name the same temperature, the same rest time and the same band convention, plus or minus or total, because the guide that publishes the table does not say which it is.

For one to a few hundred plastic parts with a handful of tight features, low-volume plastic CNC followed by bridge production is where a first article on the real grade shows which of those features hold, before the tolerance is repeated across a run.

Sources and Further Reading

Request a Plastic CNC Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Plastic CNC chosen.

Request a Quote