Two data sheets for the same family of acetal put the heat deflection temperature at 110 °C (230 °F) on one and 125 °C (257 °F) on the other, and both are correct. They differ because one is for copolymer and one for homopolymer, and because a test that bends a bar until it moves a quarter of a millimeter gives a different answer for every bar, every load and every heat history.
That quarter millimeter is ASTM D648, the test behind the letters HDT on nearly every engineering plastic sheet. Buyers of machined parts meet the number constantly and use it for a purpose the standard rules out. The sections below read what the test measures, what it was built to do, and what it leaves for the buyer to decide.
What ASTM D648 Measures
The scope of ASTM D648 is one sentence long. It covers the determination of the temperature at which an arbitrary deformation occurs when specimens are subjected to an arbitrary set of testing conditions. The standard applies to molded and sheet materials available in thicknesses of 3 mm (1/8 in) or greater that are rigid or semirigid at normal temperature, and allows stock between 1 mm and 3 mm to be tested as a composite sample at least 3 mm thick.
Two words in that scope carry the meaning: arbitrary and conditions. The test does not find the temperature at which a plastic fails. It finds the temperature at which a bar under a fixed bending load has moved by a fixed amount while the bath around it heats at a fixed rate.
A summary by the Polymer Innovation Blog describes the procedure. The bar is loaded edgewise as a simple beam. Its load is calculated for a fiber stress of 0.455 MPa (66 psi) or 1.82 MPa (264 psi).
Bath temperature rises in a heat-transfer fluid warmed at 2 ± 0.2 °C per minute, typically mineral oil up to 115 °C and silicone oil up to 260 °C. When the bar has deflected 0.25 mm (0.010 in), the bath temperature is the heat deflection temperature. The blog says at least two samples are run, the average is reported, and the stress level should be stated with the result.
The standard’s own warnings frame how the figure may be used. ASTM writes that the test is particularly suited to control and development work and that its data are not to be used to predict the behavior of plastics at elevated temperatures, except where time, temperature, method of loading and fiber stress are similar to those of the test. The data are not intended for use in design or for predicting endurance at elevated temperatures.
HDT answers one question: at what bath temperature does a standard bar under a standard load move 0.25 mm. The standard says its figure is not for design or for predicting endurance.
The Two Stress Levels Printed on Data Sheets
Every HDT on a stock sheet belongs to a load. Sheets print the pair as “at 66 psi” and “at 264 psi,” and metric sheets print 0.45 and 1.8 MPa.
| Stress | Metric | Inch | Reads as |
|---|---|---|---|
| Low | 0.455 MPa (about 0.45) | 66 psi | temperature at which the bar gives under a light load |
| High | 1.82 MPa (about 1.8) | 264 psi | temperature at which the bar gives under a heavy load |
The high-stress figure is the lower number, because a heavier load moves a hot bar sooner. A material that reads 125 °C at 264 psi may read 169 °C at 66 psi. The gap between the pair is a rough indicator of how much load the bar can carry as it warms.
A material that holds up under 1.82 MPa until a temperature close to its 0.455 MPa figure keeps its stiffness up the temperature scale. One with a wide gap loses it early.
A stock-shape sheet that prints only one value leaves the reader unable to tell which stress was used. The blog’s advice is plain: when presenting HDT data, note the stress level used in the test.
The metric and inch pairs are the same two loads in different units. A sheet that prints 1.8 MPa and 0.45 MPa is rounding the standard’s 1.82 and 0.455 MPa, and a sheet that prints 264 and 66 psi is quoting them in inch units. Set a metric sheet beside an inch sheet and the tests are the same, and a difference of a few degrees between them is the lot and the maker, not the unit.
ASTM adds that for many materials a specification may require this method with procedural modifications that take precedence, and advises reading the material specification before applying the test. A sheet written for a specified material may therefore follow the specification’s version of the procedure, and a buyer who needs the exact conditions has to ask for them.
HDT Values on Plastic Stock Data Sheets
Table 2 collects values from the sheets used in these resources, each with the load and the conditions the sheet gives.
| Sheet and material | At 1.82 MPa (264 psi) | At 0.455 MPa (66 psi) | Conditions printed |
|---|---|---|---|
| Ensinger, TECAFORM AD acetal homopolymer (Delrin 150 series) | 125 °C (257 °F) | 169 °C (336 °F) | product page values |
| Ensinger, TECAFORM AH acetal copolymer | 110 °C (230 °F) | 158 °C (316 °F) | product page values |
| Spartech, SP-1010 HDPE sheet | not listed | 80 °C (176 °F) | sheet |
| Mitsubishi, TIVAR 1000 Virgin UHMW-PE | 42 °C (ISO 75); 47 °C (116 °F) (ASTM D648) | not listed | indicative values, specimens machined from stock |
| Ensinger, TECAPEI natural, unfilled PEI | 201 °C (394 °F) | 210 °C (410 °F) | product page values |
| Ensinger, TECAPEI GF30, 30 % glass PEI | 209 °C (409 °F) | 212 °C (414 °F) | 1/4 in (6.35 mm) specimen printed |
The acetal rows show the first lesson. Four sheets cover two chemistries and give 104, 110, 121 and 125 °C at the same load, with the low-stress pair spread from 158 to 169 °C. The two chemistries sit 15 to 17 °C apart in the two copolymer and homopolymer pairs the sheets allow, and two sheets of one chemistry still differ by 4 to 6 °C. That spread is the size of the noise a buyer should expect when one sheet is swapped for another of the same polymer, and a sheet-to-sheet gap smaller than that says nothing about the bar.
The PEI rows show the second. Unfilled PEI sits within 4 °C of itself across three sheets at the high load, and 30 percent glass pushes the high-stress value up by about 10 °C and closes the gap between the two loads to 2 °C. The glass-filled bar holds its stiffness to a temperature the unfilled one reaches only at light load.
The HDPE row is a reminder that sheets do not always print both loads, and that a missing load makes a comparison between sheets unsafe.
The sheets print an HDT and a service temperature side by side, and the two differ. Service figures run 20 to 40 °C lower for acetal and about 30 °C lower for PEI.
HDT Is Not a Service Temperature
The same sheets print a service temperature, and the two numbers do not agree.
- Acetal homopolymer, TECAFORM AD: HDT of 125 °C at 1.82 MPa, long-term service temperature of 85 °C (185 °F), intermittent 149 °C (300 °F).
- Acetal copolymer, TECAFORM AH: HDT of 110 °C at 1.82 MPa, long-term service of 91 °C (195 °F), intermittent 141 °C (285 °F).
- Unfilled PEI, TECAPEI natural: HDT of 201 °C at 1.82 MPa, long-term service of 170 °C (338 °F), short-term 200 °C (392 °F).
- UHMW-PE, TIVAR 1000: HDT of 42 to 47 °C at 1.82 MPa, with a continuous service temperature in air of 80 °C (180 °F) over 20,000 hours, set where the tensile strength has fallen by about half.
The pattern repeats. Long-term service sits 20 to 40 °C below the HDT for acetal, about 30 °C below for PEI, and the UHMW-PE sheet’s maximum operating temperature is already as high as the HDPE sheet’s HDT, two different grades that show how little room polyethylene leaves. The sheets give no formula that connects the pair, and the standard says it should not be used to predict behavior at elevated temperatures.
Time is the missing variable. D648 lasts as long as the bath takes to warm, a matter of tens of minutes. A part in service sits at temperature for months, and plastics creep under load as hours pass. The test cannot see that.
For a buyer the working rule is to treat HDT as a ranking. A material with an HDT of 200 °C belongs in a hotter group than one with 100 °C, and neither figure says how long a loaded part will keep its shape at either temperature.
Conditions Behind an HDT Figure
Three conditions travel with the number, and a sheet that drops them leaves the figure ambiguous.
The first is thickness. D648 applies to stock 3 mm (1/8 in) or thicker, and Ensinger prints its glass-filled PEI deflection temperatures for a 1/4 in (6.35 mm) specimen. A thinner machined section is not what the bar tested, and the standard’s composite-specimen allowance does not make it so.
The second is heat history. Annealing is the one treatment that changes HDT by relieving residual stress, and stock shapes carry their own: Ensinger’s catalog states that its stock is annealed after production to reduce internal tension, and Mitsubishi’s guide notes that extrusion, molding and machining can leave residual stresses that redistribute when material is removed or the part sees elevated temperatures. A bar that was annealed before testing and a bar that was not may not read the same, and the sheets do not say which theirs was.
The third is the test standard. ASTM D648-18 carries a note that the standard and ISO 75-1 and ISO 75-2 address the same subject matter but differ in technical content, and that results shall not be compared between the two test methods. Earlier editions, D648-00a and D648-06, noted that D648’s Method B and ISO 75 methods Ae and Be were technically equivalent. A sheet that cites a standard by number but not by edition leaves the reader to guess which note applied.
Makers’ sheets add their own disclaimers to the figure. Mitsubishi’s TIVAR sheet says its values are mainly for comparison, are not guaranteed and are not to be used as specification limits or alone as a basis of design, and Ensinger says its values are guidelines and not minimum or maximum values. A buyer who wants a minimum has to ask for one in writing.
A Worked Reading for a Part at 80 °C
Suppose a bracket will sit at 80 °C (176 °F) in air under a steady load, and three stocks are on the table. The sheets in Table 2 and the service lines above give the first pass.
Unfilled PEI has an HDT of 200 to 204 °C at 1.82 MPa and a continuous service temperature of 170 °C, so 80 °C is far inside both. Acetal copolymer shows an HDT of 110 °C at the same load and a long-term service temperature of 91 °C. The 80 °C bracket sits 11 °C below that long-term figure and 30 °C below the HDT, a thin margin for a part that will creep. Polyethylene is out, because the HDPE sheet gives an HDT of 80 °C at the lighter 0.455 MPa load and the UHMW-PE sheet gives a maximum operating temperature of 82 °C.
The reading is a ranking. PEI has room, acetal has little, polyethylene has none. The sheets say nothing about how many months the acetal bracket holds its shape at 80 °C, and the standard says they cannot.
HDT Beside Annealing and Machining Heat
Annealing temperatures give an instructive comparison, because annealing is the one shop operation that deliberately sits near a material’s heat limit. Mitsubishi’s annealing table lists a hold of 155 °C for POM-C and POM-H, 130 °C for PE-UHMW and 200 °C for PEI. Set against Table 2, the acetal hold of 155 °C is below the 158 to 169 °C that the low-stress figures give, and the PEI hold of 200 °C matches the PEI high-stress HDT of 200 to 204 °C. The cycles heat slowly, at 10 to 20 °C per hour, and the guide advises fixturing the part through the cycle, a very different load from the 1.82 MPa a D648 bar carries.
The practical reading is that the annealing temperature of a material sits near the top of its thermal range and well above its service temperature, which is why a bar’s HDT and a shop’s oven setting are close cousins and neither is a limit on service.
Machining brings its own heat. Tangram’s guide says plastics soften at lower temperatures and conduct heat poorly, so a cutting edge concentrates heat near the surface it works on. HDT says nothing about that local heat. A cut that rubs can soften a skin of polyethylene at temperatures far below a bar test result for the bulk material.
Writing an HDT Requirement on a Drawing
When a part has to survive heat, an HDT figure is a poor requirement and a useful hint. A drawing that states the service temperature, the load and the time is stronger. If HDT is the reference, the call-out has to carry the same conditions the sheet does.
- The test standard and its edition: ASTM D648-18, or the ISO 75 part, not “HDT” alone.
- Fiber stress: 0.455 MPa (66 psi) or 1.82 MPa (264 psi).
- Specimen thickness, at least 3 mm for the standard.
- Annealed or not.
- Maker’s grade, since a different grade of the same polymer reads differently.
A complete line reads like this: heat deflection temperature, ASTM D648-18, 1.82 MPa, specimen 6.35 mm thick, annealed, minimum 200 °C, as stated by the grade’s maker. Each clause closes one of the ambiguities listed in Table 3 below, and a supplier can answer it by pointing at a maker’s sheet or by saying that the sheet does not carry the condition.
| Question | Why it changes the answer |
|---|---|
| Which stress | acetal reads 44 to 48 °C apart between 1.82 and 0.455 MPa on these sheets, PEI about 10 °C |
| Which thickness | the standard needs 3 mm or more, and thin sheets use composites |
| Annealed or not | residual stress is relieved by annealing |
| ASTM or ISO | D648-18 says results shall not be compared with ISO 75 |
| Typical or guaranteed | makers’ sheets call their values typical, for comparison |
For a heat-exposed part in a run of one to a few hundred pieces, low-volume plastic CNC followed by bridge production is best served by a drawing that states the service condition, so the supplier can pick a grade and a stress-relief step to match it.
Heat deflection is one temperature on the sheet, and the others move with it. Ensinger’s unfilled PEI deflects at 201 °C (394 °F) at 1.82 MPa, while its linear thermal expansion of 56 x 10⁻⁶ per K says how far a part grows on the way there and its tensile modulus of 2.96 GPa (430,000 psi) by ASTM D638 is a room-temperature figure that falls as the part warms. A machined part cut from rod or plate inherits all three, and a drawing that names a service temperature asks for the deflection, the growth and the stiffness at that temperature together.
Sources and Further Reading
- ASTM International, ASTM D648-18, Standard Test Method for Deflection Temperature of Plastics Under Flexural Load in the Edgewise Position, active
- ASTM International, ASTM D648-06 listing, historical
- Polymer Innovation Blog, Heat deflection temperature, ASTM D648
- Ensinger, TECAFORM AD natural, POM-H, product data and TECAFORM AH natural, POM-C, product data
- Ensinger, TECAPEI natural, product data and TECAPEI GF30 natural, product data
- Ensinger, Stock Shapes catalog, 2024
- Mitsubishi Chemical Group, TIVAR 1000 Virgin UHMW-PE, product data sheet, 2026
- Spartech, SP-1010 HDPE technical data sheet
- Mitsubishi Chemical Advanced Materials, Guide to machining plastic parts
- Tangram Technology, Plastics Topics, Machining of plastics