AcrylicBurrInternal Stress

Inspecting a Batch of Machined Plastic Parts Before It Ships

Inspecting machined plastic means stating the temperature, the probe force and the sample size, because a plastic part changes with all three.

A batch of identical CNC machined black acetal brackets in rows, one turned over to show its underside, beside two plain unmarked steel pin gauges.

A probe that presses a polymer surface with 100 grams of force is not measuring the same part as a probe that presses it with 6 grams. Kleiss Gears, a maker of polymer gears, says so in a trade article on its measuring practice. The 100 gram probe is not significant on a metal model, in the maker’s words, while on a polymer model that much force can deform the surface and give false readings, in a world where the tolerances run under 0.025 mm (0.001 in). A batch of machined plastic parts is inspected inside the same physics, and the inspection plan has to account for it before any number goes on a report.

What follows is the order a careful inspection takes: conditioning the part, choosing the probing method, reading the first parts against the aim point, deciding how many parts to measure, judging capability honestly for small batches, and writing the record that travels with the shipment.

How to Inspect a Batch of Machined Plastic Parts

Inspect the batch at a stated temperature, with a low-force or non-contact method for soft or thin parts, on a sample whose size is chosen in advance, and record the conditions with the results. Those four elements separate a measurement that can be repeated from one that cannot.

The reasons come from the material, and the stock-shape makers state them.

MCAM, the Mitsubishi Chemical group’s advanced materials division, lists four differences between plastics and metals in its 2026 machining guide: thermal expansion up to ten times higher, slower loss of heat, much lower softening and melting temperatures, and much higher elasticity. Two more follow from the material: nylons swell as they take up moisture, and internal stress released by machining can deform a part during and after the cut. Each of these touches the inspection. Temperature changes size, softness changes what a probe does, and moisture and stress make the size drift with time.

A plastic part therefore has a measurement context in addition to a measurement, and the context is what an auditor asks to see first, before looking at any single dimension. Without the context, two labs can report two sizes for the same part and both be right.

A measurement of a plastic part is a number plus a temperature, a probe force and a time since machining. Take any of the three away and the number cannot be compared.

Conditioning the Part Before Any Number Is Taken

The reference temperature for dimensional measurement is 20 °C (68 °F). Ted Doiron of NIST traces the history in a 2007 paper in the Journal of Research of the National Institute of Standards and Technology: the International Committee for Weights and Measures adopted 20 °C unanimously on April 15, 1931, after about twenty years of discussion. Industrial lengths since then are the size at 20 °C.

A few kelvin of error is a few micrometers on a metal part. On a plastic part the same few kelvin is a different order of size. Röhm gives the linear expansion of PLEXIGLAS as 0.07 mm per meter per kelvin, and its example, 1.4 mm over 1,000 mm between 10 °C and 30 °C, ends with the instruction to check the dimensions of identical parts at the same ambient and material temperatures. Table 1 scales that coefficient to part lengths and temperature differences a shop meets between the machine, the truck and the measuring room.

Table 1. Length change of acrylic for a temperature difference from 20 °C, from the Röhm coefficient of 0.07 mm/(m·K)
Length, mm (in) 2 K off, mm 5 K off, mm 10 K off, mm
50 (2.0) 0.007 0.018 0.035
100 (3.9) 0.014 0.035 0.070
250 (9.8) 0.035 0.088 0.175

Acrylic is the case Röhm documents. Other polymers have their own coefficients on their datasheets, and the point is the scale: a 100 mm part 5 K off the reference temperature moves by 0.035 mm, which is comparable to the 0.05 mm (0.002 in) that MCAM’s standard tolerance curve holds for sizes up to about 50 mm. Parts therefore sit in the measuring room until the core of the part and the room are the same temperature, and the room itself is held near 20 °C.

Deburring comes before measurement, and it is a measuring condition of its own. MCAM names sharp knives or rotating hooks as the most common tools and stresses tool sharpness, with countersink tools that do not cut too deep or chatter, wet and dry abrading for hard plastics, rotary stones for some, and hot air for complex profiles in general engineering plastics. A burr left on a bore edge lifts a probe, and a burr removed with a dull tool changes the edge it measures.

Moisture is the second condition.

A nylon part that has taken up moisture grows, and the change can be reversed by drying. A part measured at the end of a humid week is not the part that left the machine. The record states whether the part was measured as machined, after drying or after conditioning. Conditioning in either direction is slow, since water moves through a thick wall over days.

Time since machining is the third. MCAM’s advice to rough and then rest for 24 hours shows that stress relief works over days. A part measured an hour after the finishing cut and again a week later can differ, and the report says which it is.

Probe Force and Soft Parts

A touch probe pushes on the part. For soft or thin parts the deflection is part of the reading, and the Kleiss article states the practical limit in grams.

In metal gearing probe force is not a factor, the authors say, but with polymers probe sizes are smaller and the force can approach the deformation point of the part. A polymer force model can be as small as 6 grams, and measuring with 6 grams and with 100 grams gives two different measurements in the sub-0.025 mm range. The same article notes that the equipment and software of many manufacturers may not address force properly, and that below a certain feature size optical methods have to replace probes.

Four conditions follow for an inspection plan:

  • name the probe tip diameter and the trigger or scanning force used on the soft features;
  • measure thin walls and flexible edges with an optical or video method when the probe deflects them;
  • support the part on the same datum faces the machine used, so that gravity bends it the same way;
  • keep the clamping force on the measuring fixture as low as the machining clamping force, for the reasons given in the workholding piece in these resources.

The same logic applies to the datum scheme: a part that is clamped on its own datum faces at the measuring station sits as it sat on the machine, and a part measured freely on a flat plate can sag by a different amount. None of this needs a particular instrument. It needs a statement in the plan of how force and support are controlled, and that is what an auditor of a plastic part looks for.

First Parts and the Aim Point

A first part is cut, measured, and used to correct the program. MCAM’s turning tips give two instructions for this loop: most diameters grow after cutting, so aim for the lowest dimension in the band when setting, and consider capability studies on the machines. Together they describe the aim point, which is where in the tolerance band the program is set to run.

On a tolerance of 0.1 percent of the dimension, a 100 mm (3.9 in) feature carries plus or minus 0.1 mm (0.004 in).

The band itself is wider for plastic than for metal. MCAM prints its best machining tolerances by size and material group, and notes that such extra-precise tolerances can need special tooling and extra steps. For PA and POM the best is 0.04 mm (0.0016 in) at 25 mm and 0.15 mm (0.006 in) at 200 mm, and its standard curve stays flat at 0.05 mm (0.002 in) up to about 50 mm and climbs to about 0.15 mm near 150 mm.

Features that drift are the ones worth re-measuring. MCAM’s annealing pages name the parts where internal stress relief shows most: large or asymmetrical parts and those with substantial material removal, such as a U-shape cut from a plate or a bush bored from solid rod. On a part like that, the plan measures flatness across the open side, the width of the slot and the roundness of the bore on the first part and again after the rest, and on later parts it keeps only the features that moved.

Features that stay put through the rest do not need the same attention in every later batch, while one that moves by a third of its tolerance does, and the plan says so. The decision is written down with the measured movement beside it, so that a later change of stock lot or of cutter can be judged against the first record. A shop that keeps these first-part movements on file can tell a normal rest from an abnormal one without guessing. The aim is a measurement load that follows where the part changes, not an equal share of effort on every dimension.

The first-part loop answers one question: where does the process sit relative to the band. Later parts answer another: does it stay there. An inspection plan keeps the two apart, with the first part measured fully and later parts measured on the features that drift.

Sampling Plans for a Small Batch

A batch of machined parts is small enough that the choice between measuring all of it and sampling it is a real one.

The NIST Engineering Statistics Handbook describes the standard ways to decide.

A lot acceptance sampling plan is a sampling scheme and a set of rules for making decisions. In the single sampling plan, usually written (n, c), one random sample of n items is taken and the lot is rejected if there are more than c defectives. The handbook calls this the most common and the easiest to use, though not the most efficient in the average number of samples. Double, multiple, sequential and skip-lot plans extend the idea.

The plan carries a risk that a buyer should see in numbers. Table 2 computes the probability that a plan accepts a lot, from the binomial distribution, for lots with different true defect rates. The calculation treats the lot as large relative to the sample, which is an approximation for batches of a few hundred parts.

Table 2. Probability of accepting the lot, percent, for four single sampling plans (n, c), binomial approximation
Plan (n, c) Lot 1 % defective Lot 2 % defective Lot 5 % defective Lot 10 % defective
(8, 0) 92 85 66 43
(20, 0) 82 67 36 12
(32, 1) 96 87 52 16
(50, 1) 91 74 28 3

The table shows that a plan of 8 parts with no defects allowed accepts a lot that is 10 percent defective more than 40 percent of the time. A plan of 50 parts allowing one defect accepts it 3 percent of the time. The sample size, not the batch size, sets this protection.

The handbook also describes skip-lot plans, in which only a fraction of the submitted lots is inspected. That suits a repeat order from a supplier whose first lots passed with a good record, and it does not suit the first order of a new part, where every lot is the first evidence the buyer has, and where a sample drawn from it carries the whole decision.

Two consequences matter for a buyer. A small sample accepts poor lots often, so the sample is sized to the risk the program can tolerate. And a feature that matters for fit, such as a bore for a bearing, is measured on every part, since a plan that allows a defect on that feature is not a plan for that feature.

Capability Needs More Parts Than a Small Batch Has

Process capability indices compare the spread of a process to the specification width. NIST defines them in its handbook: Cp is the specification width divided by six standard deviations, and Cpk is the smaller distance from the mean to either specification limit divided by three standard deviations. The handbook notes that most estimates are valid only if the sample is large enough, which is generally thought to be about 50 independent data values, and that the indices assume normally distributed data.

An illustration with assumed numbers shows what the index tells.

A feature has a tolerance of plus or minus 0.10 mm (0.004 in) and a standard deviation of 0.02 mm. Cp is 0.20 divided by 0.12, which is 1.67. If the mean sits 0.03 mm off center, Cpk falls to 1.17. The index says that centering is the thing to fix, and it says it only when the standard deviation is known.

For a batch of 30 or 40 parts, the standard deviation has a wide confidence interval and the index is a rough guide. A plan that reports Cpk on a batch of that size should state the sample size next to it. MCAM’s recommendation to run capability studies on the machine points the same way: the study is done once on the machine with enough parts, and later batches rely on it.

Release Checks Before the Parts Are Packed

Inspection ends with release, and for plastic the packing step belongs to it, since the part keeps changing after it leaves the room. The makers’ documents give the items:

  • Nylon parts that carry a tight size are packed against moisture, so they reach the customer at the size they were measured.
  • Amorphous parts machined with coolant, such as polycarbonate, PSU, PPSU and PEI, are washed in isopropyl alcohol and rinsed in pure water before release, which MCAM gives as the protection against stress cracking.
  • Acrylic parts keep their masking film until they are in place. Röhm lists other protection for machined sheet and parts, among them strippable coatings such as a 30 percent aqueous solution of PVAL, compatible adhesive crêpe tapes and closed polyethylene bags.
  • Parts that were annealed or post-cured leave with the cycle noted, since a post-cured polyamide-imide part keeps a surface layer that a later cut would remove.

Each item takes minutes and protects a dimension that was expensive to reach. A shipment that arrives with its moisture state or its surface intact shows the same numbers at the customer that the inspection report shows.

A plastic part is not finished at the last cut. It is finished when it leaves the measuring room in a state that matches its report.

What the Record Carries to the Customer

The record is the last product of the inspection. For a plastic part it carries more than dimensions, because the context decides how the dimensions are read. Table 3 lists the items and the reason each one is there.

Table 3. Items in an inspection record for machined plastic parts
Item Reason it is recorded
Stock grade, maker and lot Separates a material effect from a process effect; stock shapes carry their own history of stress relief
Heat treatment performed Rest, anneal or post-cure change the size and the stability
Measurement temperature and soak time The 20 °C reference and the large expansion of plastic
Probe, tip and force, or optical method Soft parts deflect under contact force
Sample size and plan The risk of accepting a poor lot depends on it
Moisture state and packaging Nylons, PBI and PAI swell and shrink with moisture
Features measured on all parts Fit-critical features are not sampled

A record built this way travels. The record lets an incoming inspection reproduce the measurement, lets a molder compare machined and molded parts, and lets a later batch be compared with the first. It is also the document a buyer needs when planning low-volume plastic CNC work that has to continue under bridge production with the same acceptance basis.

Sources and Further Reading

Request a Plastic CNC Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Plastic CNC chosen.

Request a Quote