One cast nylon, two data sheets, two hardness values: Röchling prints Shore D 83 for Sustamid 6G natural on its ISO sheet and Shore D 78 for Sustamid 6G on its ASTM sheet. The polymer is the same family from the same maker. Its test standards are not, and neither is the specimen preparation behind them. A buyer comparing a supplier’s substitute against the original grade by its hardness line can therefore find a five-point gap that says nothing about the plastic.
Hardness is one of the most visible rows on a plastic stock data sheet and one of the easiest to misread. It appears in two forms, Shore D from a durometer and Rockwell from an indentation tester, under two families of standards, ASTM and ISO. This article reads the public scopes of the ASTM methods, sets the values the stock makers actually print side by side, and explains what the numbers do and do not commit a supplier to.
What Shore D and Rockwell Numbers Mean on a Plastic Stock Data Sheet
Both numbers rank how strongly a plastic resists a hard indenter pressed into its surface at room temperature. Neither is a strength, a wear rating or a design value. ASTM states this plainly for both methods.
For durometer hardness, ASTM D2240 calls the test empirical and intended primarily for control purposes, with no simple relationship to any fundamental property of the material. On the Rockwell side, ASTM D785 says the results are not generally considered a measure of abrasion or wear resistance.
The two scales differ in what they press and how they read it. Shore D comes from a durometer, which measures the penetration of a specified indentor under specified conditions, and the reading is higher when the penetration is smaller. A Rockwell tester, by contrast, measures the net increase in depth of an impression as a ball indenter goes from a small load to a large load and back. Among the Rockwell scales, M and R are the ones printed most often for engineering plastics.
A hardness value on a plastic data sheet is a quality-control number from a standard specimen. It ranks materials and checks consistency, but it does not predict wear, strength or service behavior.
ASTM D785, Rockwell Hardness of Plastics
ASTM D785 is the standard test method for Rockwell hardness of plastics and electrical insulating materials. Its public scope describes two procedures, and both use round steel ball indenters of specified diameters.
- Procedure A reads the indentation that remains 15 seconds after the major load is released back to a standard 10 kg minor load. Its result is the Rockwell hardness number.
- Procedure B reads the indentation while the major load is still applied, after 15 seconds. Its result is the Rockwell alpha (α) hardness number, equal to 150 minus the instrument reading.
Each Rockwell scale division corresponds to 0.002 mm (0.00008 in) of vertical movement of the indenter. ASTM gives the relationship between the hardness number and the depth of impression for the E, M, L, R and K scales, and states that a higher reading means a harder material. Every Rockwell number is quoted with its scale symbol, which identifies the indenter size, the load and the dial scale used.
Three cautions from the same scope matter on a data sheet. The scales overlap at their ends, so a single material can give two technically correct readings on two scales. Creep and recovery in some plastics make the timing of the loads affect the result considerably. And a correlation table between scales is described as not desirable, because readings that line up for one plastic may not line up for another with different elasticity, creep or shear behavior.
ASTM names ISO 2039-2 as the equivalent international method. Procedure A matches the main body of ISO 2039-2, and Procedure B matches its annex.
ASTM D2240, Durometer Hardness and the Shore D Scale
ASTM D2240 covers twelve types of durometer: A, B, C, D, DO, E, M, O, OO, OOO, OOO-S and R. The method is written for thermoplastic elastomers, vulcanized rubber, elastomeric and cellular materials, gel-like materials and some plastics. Type D is the one behind the Shore D values printed on plastic stock data sheets.
The scope sets clear limits on comparison. Indentation hardness depends on the elastic modulus and viscoelastic behavior of the material, and the indentor geometry and force shape the result, so there is no simple relationship between one durometer type and another or between a durometer and other hardness instruments. ASTM adds that D2240 is not equivalent to other indentation hardness methods and that instruments for mass, force and dimension are to be traceable to a national standards body.
European data sheets print Shore D to DIN EN ISO 868. The ISO text itself is not public, so its details are not reproduced here. What a buyer can take from the sheets is that the ISO and ASTM methods are different documents, and that the same maker reports different Shore D values for the same grade under each.
Table 1 collects what the public pages and the data sheets print about the methods behind the hardness rows.
| Method | What it reads | Classes or scales named | Equivalence stated |
|---|---|---|---|
| ASTM D785, Procedure A | Remaining depth 15 s after the major load is removed to a 10 kg minor load | Rockwell scales E, M, L, R, K | Main body of ISO 2039-2 |
| ASTM D785, Procedure B | Depth after 15 s under the major load; α = 150 minus reading | Rockwell α | Annex of ISO 2039-2 |
| ASTM D2240 | Penetration of a specified indentor; higher reading, smaller penetration | Twelve durometer types, A to R; type D is the one stock sheets print as Shore D | Not equivalent to other indentation methods |
| DIN EN ISO 868 | Shore D as printed on European stock sheets | Shore D | Not stated on the sheets |
Hardness Values Printed on Engineering Plastic Stock
Table 2 lists the hardness values that Ensinger and Röchling print for common machining grades. The method column is copied from each sheet. Where a sheet prints a Rockwell number without a scale letter, the table says so rather than guessing the scale.
| Grade (maker) | Shore D, method | Rockwell, method |
|---|---|---|
| TECAPEEK natural, unfilled PEEK (Ensinger, US data) | 88, ASTM D2240 | M 100 and R 125, ASTM D785 |
| TECAPEEK natural, unfilled PEEK (Ensinger, European data) | 89, DIN EN ISO 868 | not printed |
| TECAPEEK CF30 black, 30 % carbon fiber PEEK (Ensinger) | 90, DIN EN ISO 868 | not printed |
| TECAFORM AH natural, acetal copolymer (Ensinger, US data) | not printed | R 120, and 86 with no scale printed, ASTM D785 |
| Sustamid 6G, cast PA6 (Röchling, ASTM sheet) | 78, ASTM D2240 | R 115, and 85 with no scale printed, ASTM D785 |
| Sustamid 6G natural, cast PA6 (Röchling, ISO sheet) | 83, DIN EN ISO 868 | not printed |
| TECAMID 6 natural, extruded PA6 (Ensinger) | 79, DIN EN ISO 868 | not printed |
| Polystone M Flametech AST black, flame-retardant UHMW-PE (Röchling) | above 63, DIN EN ISO 868 | not printed |
Three readings follow from the table. The Shore D values of the rigid engineering plastics crowd into a narrow band, from 78 to 90, so Shore D separates nylon from PEEK but says little between grades of one family. Rockwell R values, meanwhile, crowd at the top of the scale, from 115 to 125, which is why harder plastics also carry an M-scale value: PEEK reads M 100 on the more severe scale. And UHMW-PE sits clearly lower, above Shore D 63, which matches its softness at the cutter and its tendency to burr.
Carbon fiber barely moves the surface reading. TECAPEEK CF30 black reads Shore D 90 against 89 for the unfilled grade, although its tensile modulus on the same sheets is about 40 % higher. Surface hardness and stiffness answer different questions.
Conditions the Sheets Do Not Print
None of the sheets in Table 2 states the specimen thickness, the conditioning or the moisture state behind its hardness value. For most grades that matters little at room temperature. Nylon is the exception, because Röchling notes under its PA6 table that moisture absorption changes the mechanical properties: the material becomes tougher and its modulus falls, while thick sections change only in a surface layer. A hardness reading taken on a dry bar and one taken on a conditioned bar are therefore not guaranteed to agree, and the sheet alone does not say which state its number describes.
ASTM D785 puts the order of authority in writing. Before the method is used, the material specification is to be consulted, and any specimen preparation, conditioning, dimensions or test parameters it sets take precedence over the defaults in the test method. The scope adds one more use of indentation hardness that is outside machining stock but explains the method’s origin: on thermosetting materials, a reading below normal can indicate an incompletely cured specimen.
Why Shore D and Rockwell Cannot Be Converted
Buyers often ask for a conversion between a Shore D value and a Rockwell value, or between Rockwell M and R. The standards themselves argue against it. ASTM D785 describes a correlation table between Rockwell scales as not desirable, and ASTM D2240 states that no simple relationship exists between durometer readings and other hardness instruments.
The Röchling sheets show the same limit within one scale. Sustamid 6G reads Shore D 78 under ASTM D2240 and Shore D 83 under DIN EN ISO 868 for cast PA6 of the same family. A conversion from one method to the other would have to absorb that difference, and the difference itself depends on the material.
The practical rule for a specification is simple.
- Name the method and the scale with the number: Shore D to ASTM D2240, Shore D to ISO 868, Rockwell M or R to ASTM D785.
- Compare grades only on the same method and scale.
- Treat a Rockwell value printed without its scale letter as incomplete, and ask the supplier which scale it is.
- Do not use hardness as a stand-in for wear resistance, which D785 rules out explicitly.
A hardness number without its method and scale is not a specification. With them, it is a useful check that the bar on the saw is the grade on the drawing.
Heat Deflection Temperature Beside Hardness
Hardness is measured at room temperature, which is one reason it says little about a part that runs warm. The row that addresses temperature on the same data sheets is heat deflection temperature (HDT), measured to ASTM D648 or ISO 75. Hardness and HDT belong together in a review because both are short-term tests on a standard specimen.
ASTM’s public scope for D648 describes the test as finding the temperature at which an arbitrary deformation occurs under an arbitrary set of test conditions. It applies to molded and sheet materials 3 mm (0.125 in) or thicker that are rigid or semirigid at normal temperature. The data are suited to control and development work and, in ASTM’s words, are not intended for design or for predicting endurance at elevated temperatures. ASTM also states that D648 and ISO 75-1 and 75-2 differ in technical content and that results from the two are not to be compared.
| Grade (maker) | HDT, method and stress | Value |
|---|---|---|
| TECAPEEK natural (Ensinger, US data) | ASTM D648, 1.82 MPa (264 psi) | 160 °C (320 °F) |
| TECAPEEK natural (Ensinger, European data) | ISO 75, method A | 162 °C (324 °F) |
| TECAFORM AH natural (Ensinger, US data) | ASTM D648, 1.82 MPa (264 psi) | 110 °C (230 °F) |
| TECAFORM AH natural (Ensinger, US data) | ASTM D648, 0.45 MPa (66 psi) | 158 °C (316 °F) |
| Sustamid 6G (Röchling, ASTM sheet) | ASTM D648, 1.82 MPa (264 psi) | 91 °C (195 °F) |
| Sustamid 6G (Röchling, ASTM sheet) | ASTM D648, 0.45 MPa (66 psi) | 188 °C (370 °F) |
| Sustamid 6G natural (Röchling, ISO sheet) | ISO 75, method A | 95 °C (203 °F) |
The pairs in the table show the same pattern as the hardness rows. Each grade carries different values under ASTM and ISO, and the stress level changes the result far more than the method does. Sustamid 6G deflects at 91 °C (195 °F) under 1.82 MPa (264 psi) and at 188 °C (370 °F) under 0.45 MPa (66 psi). An HDT value without its stress level is as incomplete as a Rockwell value without its scale.
Hardness and HDT are both short-term readings on standard specimens. Each needs its method and its scale or stress printed beside it before two grades can be compared.
Where a sheet prints no HDT, it sometimes prints another short-term softening value. Röchling gives a Vicat softening temperature of 79 °C (174 °F) to DIN EN ISO 306, method B, for its flame-retardant UHMW-PE, which is a different test with its own load and its own meaning.
What a Data Sheet Value Commits the Supplier To
A data sheet is information, not a certificate. Röchling states on its sheets that the values are averages determined by statistical tests on a regular basis, provided for information only and not binding unless expressly agreed in a contract of sale. Its ISO sheet adds that properties depend on the dimension of the semi-finished product and its degree of crystallization, so the values of a particular product may differ from those printed. The ISO sheet also states that its values follow DIN EN 15860, the European standard for thermoplastic semi-finished products for machining.
Ensinger draws the same line from the other side. It issues material confirmations only in connection with an actual order and the material supplied, and it can carry out tests in its own laboratories as part of a works test certificate of type 3.1 to EN 10204, by agreement at the time of order.
For a buyer, that leaves a short list of what to write when hardness or HDT matters to the part.
- The property, the method and the scale or stress, for example Rockwell M to ASTM D785 or HDT to ASTM D648 at 1.82 MPa.
- Whether the value is a typical value for identification or a tested value for each lot.
- If it is tested, the certificate type, such as EN 10204 3.1, and the lot it covers.
- The specimen source, from the delivered stock shape or from the maker’s standard specimen.
The last point matters most. A hardness check on the delivered bar is a good receiving test for confirming the grade. It is not the same number as the one on the sheet, which comes from a standard specimen prepared under the method’s own conditions.
For machined parts where the grade has to be confirmed lot by lot, low-volume plastic CNC with bridge production carries the stock certificate and the stated test method from the material lot to the finished batch.
Sources and Further Reading
- ASTM D785, Standard Test Method for Rockwell Hardness of Plastics and Electrical Insulating Materials, ASTM International
- ASTM D2240, Standard Test Method for Rubber Property, Durometer Hardness, ASTM International
- ASTM D648, Standard Test Method for Deflection Temperature of Plastics Under Flexural Load in the Edgewise Position, ASTM International
- PEEK unfilled, TECAPEEK natural (US data), Ensinger
- PEEK unfilled, TECAPEEK natural (European data), Ensinger
- PEEK carbon fibre reinforced, TECAPEEK CF30 black, Ensinger
- POM-C unfilled, TECAFORM AH natural, Ensinger
- PA 6, TECAMID 6 natural, Ensinger
- Frequently asked questions, machinable plastics, Ensinger
- Technical Data Sheet, Sustamid 6G, ASTM, version 2.0, 2024, Röchling
- Technical Data Sheet, Sustamid 6G natural, version 4.0, 2023, Röchling
- Technical Data Sheet, Polystone M Flametech AST black, version 3.0, 2025, Röchling