AcetalHDPEThickness

ASTM D638 Tensile Strength on Plastic Stock Data Sheets

A tensile figure on a data sheet belongs to one bar, one speed and one reading, so the sheet has to name all three before the number guides a design.

Machined dog-bone tensile test bars in white acetal, black acetal and natural cream nylon, plain and unmarked, one bar pulled apart with a necked and broken middle.

One UHMW-PE bar from one maker prints a tensile strength of 40.0 MPa (5,800 psi) in its ASTM column and 19 MPa in its ISO column, on the same data sheet. Neither number is wrong: one is the ASTM D638 result, which the sheet pairs with an elongation at break, and the other the ISO 527 result, which it pairs with an elongation at yield, on a different bar and at a different speed. A buyer who wants to know the strength of a part has to know which one is being quoted.

All three come from ASTM D638, and the standard says in its own notes why the numbers move. This piece reads D638 as the buyer of a machined plastic part meets it: what it covers, what the words yield and break report, which of its conditions a sheet leaves out, and what changes between the test bar and the machined part.

What ASTM D638 Covers

The scope of ASTM D638, Standard Test Method for Tensile Properties of Plastics, is the determination of the tensile properties of unreinforced and reinforced plastics in the form of standard dumbbell-shaped specimens, tested under defined conditions of pretreatment, temperature, humidity and testing machine speed. On astm.org the 2022 edition is listed as active.

The scope draws four lines that matter to a buyer of stock:

  • It applies to materials of any thickness up to 14 mm (0.55 in). Material thicker than 14 mm is reduced by machining to make the specimen.
  • Thin sheeting under 1.0 mm (0.04 in), including film, belongs to a different standard, ASTM D882.
  • Values stated in SI units are the standard, with inch units in parentheses for information only.
  • D638 and ISO 527-1 address the same subject matter but differ in technical content.

The last point is easy to miss. A sheet that prints ISO 527 values and a sheet that prints D638 values are describing different tests, and the two columns are not interchangeable.

D638 pulls a dumbbell-shaped bar under stated conditions of temperature, humidity and speed. The number it gives belongs to that bar and those conditions.

What Yield, Break and Elongation Mean on a Sheet

A tensile test draws a bar until it fails and records stress against strain. The sheets print three kinds of reading from that curve.

Yield is the stress where the bar stops springing back elastically and starts to flow. For a ductile plastic, the sheet prints a yield stress and the strain at that point. Break is the stress and strain at the moment of failure. Modulus is the stiffness in the elastic stretch before either, printed as a single number in GPa or psi.

The three can differ widely for one material. Spartech’s SP-1010 HDPE sheet prints a tensile strength of 31.0 MPa (4,500 psi) with 800 percent elongation. Mitsubishi’s TIVAR 1000 UHMW-PE sheet prints 40.0 MPa (5,800 psi) by ASTM D638 at 300 percent elongation at break, and 19 MPa by ISO 527 with 15 percent elongation at yield. A designer who reads the 40 MPa figure for UHMW-PE and designs to it will be disappointed, because the bar yields at roughly half that stress.

Elongation is a similar trap. A reading of 250 or 1,350 percent says the bar stretches to several times its length before it breaks, and that it will have changed shape long before. For a part that has to keep its shape, the yield side of the curve is the one that counts.

Tensile Values on Stock Data Sheets

Table 1 lists the D638 entries from sheets used across these resources, with the metric value first.

Table 1. D638 tensile entries on stock sheets at 23 °C (73 °F), as printed, converted to metric
Sheet and material Tensile strength, MPa (psi) Elongation, % Tensile modulus, GPa (psi)
Ensinger, TECAFORM AD acetal homopolymer 75.8 at yield (11,000) 25 at break 2.41 (350,000)
Ensinger, TECAFORM AH acetal copolymer 64.1 at yield (9,300), 66.9 at break (9,700) 9 at yield, 40 at break 2.28 (330,000)
Mitsubishi, TIVAR 1000 Virgin UHMW-PE 40.0 (5,800), ASTM D638; 19, ISO 527 300 at break (ASTM); 15 at yield (ISO) 0.55 (80,000), ASTM; 0.75, ISO
Spartech, SP-1010 HDPE 31.0 (4,500), type not stated 800 1.34 (195,000)
Ensinger, TECAPEI natural, unfilled PEI 120.7 at break (17,500) 7 at yield, 40 at break 2.96 (430,000)
Ensinger, TECAPEI GF30, 30 % glass PEI 124.1 at break (18,000) 3 at break 5.52 (800,000)

Two rows print one strength with no label for yield or break, and the Mitsubishi sheet explains why that matters: its note to the tensile line says that tensile strength may refer to either the strength at yield, with the elongation at yield reported, or the strength at break. The copolymer row shows the size of the gap, 64.1 MPa at yield against 66.9 MPa at break on one sheet. Without the label, a difference of a few MPa could be the material or the reading.

Read the UHMW-PE row twice. The same bar from the same maker prints 40.0 MPa by ASTM D638 and 19 MPa by ISO 527, and a modulus of 0.55 GPa by one method and 0.75 GPa by the other. Nothing changed but the method and the point on the curve that was reported. A comparison of two sheets is therefore a comparison of the same method and the same label, or it says nothing.

The PEI rows say the same thing from the other side. Ensinger’s unfilled TECAPEI and its glass-filled grade print break strengths 3 MPa apart, yet the unfilled bar stretches to 40 percent before it breaks and the glass-filled bar to 3 percent. Strength alone would call them alike; the elongation column says one bends and the other snaps.

Test Speed, Specimen and Thickness Move the Number

D638 states its own limits in a note. The constant-rate-of-crosshead-movement method, the standard says, leaves much to be desired from a theoretical standpoint. Wide differences may exist between the rate of crosshead movement and the rate of strain between gage marks on the specimen, and the testing speeds specified disguise important effects characteristic of materials in the plastic state.

The same note covers thickness. Variations in specimen thickness, which the procedure permits, produce variations in the surface-to-volume ratio of the specimen, and those variations may influence the results. The standard’s remedy is that where directly comparable results are desired, all samples should be of equal thickness.

Mitsubishi’s sheet is the one in Table 1 that prints its test conditions in full. Its notes give the ASTM tensile speed as 0.2 in/min or 2 in/min, chosen by whether the material behaves tough or brittle, on Type 1 tensile bars, and the ISO speed as 5 or 50 mm/min on type 1B bars, with the choice made according to ISO 10350-1. The other sheets print neither a specimen type nor a speed. A comparison of one labeled test with several unlabeled ones is a comparison of different things.

The standard’s section on engineering design carries a caution of its own. Per its scope, test data obtained by the method have been found to be useful in engineering design, but that the precautions and limitations of the method in Note 2 and in Section 4 need to be considered before using the data for design. It also states that special additional tests should be used where more precise physical data are needed.

Conversions are mechanical and worth doing before any comparison. One thousand psi is 6.895 MPa, so 11,000 psi is 75.8 MPa and 450,000 psi is 3.10 GPa. The standard states SI as its own unit, and the sheets that print only psi are quoting the inch-pound value the ASTM committee gives for information. Where two sheets differ by less than the rounding of a conversion, 0.1 MPa or so, they agree.

Mitsubishi also says where in a section its bars come from: most mechanical figures are average values of tests on dry specimens machined out of rods of 40 to 60 mm where available, otherwise out of plate of 10 to 20 mm. D638 covers material up to 14 mm thick and has thicker stock machined down, so a test bar from a 40 mm rod has been cut from somewhere inside it. ASTM D6100 lists porosity level among the properties of acetal shapes, which shows why the question is fair, since the weakest line in a bar sits along its center.

Tensile Modulus and How Far a Part Bends

For most machined parts, stiffness decides the design before strength does. The modulus on the sheet is the number that sets how far a wall or a bracket moves under a load that stays well below yield, and it is the number that moves least between sheets.

In Table 1 the unfilled acetals sit at 2.28 and 2.41 GPa, HDPE at 1.34 GPa, unfilled PEI at 2.96 GPa and TIVAR 1000 UHMW-PE at 0.55 GPa by ASTM. For two parts of the same shape and load, deflection in the elastic range scales inversely with modulus. A PEI bracket then deflects roughly a fifth as far as the same bracket in UHMW-PE, and a bracket in acetal about a quarter as far.

Ensinger’s PEI pair shows what fiber does to the numbers. At 30 percent glass the tensile modulus climbs from 2.96 to 5.52 GPa, nearly a factor of two, while the tensile strength at break moves from 120.7 to 124.1 MPa and the elongation at break falls from 40 to 3 percent. Stiffness gains far more than strength, and toughness pays for both, which is the usual trade.

Three cautions keep the arithmetic honest:

  • The modulus is read at room temperature. A part at service temperature is softer, and the HDT and service lines on the same sheets say how soon.
  • Plastics creep. Tangram lists creep under load among the properties that separate plastics from metals, and no modulus on a D638 sheet includes it.
  • Flexural modulus, the figure from a bending test, sits near the tensile figure on most sheets but not on all. Spartech’s HDPE sheet gives a flexural modulus of 1.55 GPa against a tensile value of 1.34 GPa, and Ensinger’s acetal copolymer 2.76 against 2.28 GPa, so the two cannot be swapped without a note.

Stiffness decides how far a wall bends and moves least between sheets. Strength decides when it yields and moves most, because yield, break, speed and thickness all shift it.

What Changes Between the Test Bar and a Machined Part

A D638 specimen is a smooth dumbbell pulled along its length. Machined parts have corners, holes, walls, threads and a surface the cutter left. Each of those changes the answer, and each has a source.

Table 2. Test bar compared with a machined part, each difference with its source
Feature D638 bar Machined part Source for the difference
Geometry smooth dumbbell sharp corners, holes, threads Mitsubishi’s guide lists missing chamfers at sharp corners among the causes of cracking and corner chipping
Internal condition bar machined from a 40 to 60 mm rod or a 10 to 20 mm plate centerline of rod or plate may be porous Mitsubishi’s test notes; ASTM D6100 lists porosity level as a property of acetal shapes
Residual stress not the point of the test can release when material is removed Mitsubishi and Tangram on stress relaxation after machining
Temperature 23 °C whatever the part sees HDT and service temperatures on the same sheets
Loading steady pull clamp, bolt, fastener and creep Tangram on deformation under clamp pressure and creep

Stock thicker than 14 mm, which the standard machines down into a specimen, connects the two worlds. The test bar from a thick plate is itself a machined part, cut from somewhere in the section. Which part of the section it came from, near the face or through the centerline, is not stated on a stock sheet.

The practical consequence is margin. A sheet’s tensile figure ranks materials, and a designer applies a safety factor for geometry, temperature and time that the sheet cannot give. The standard does not supply that factor, and neither do the makers.

Ensinger’s sheet gives one example of the clause worth looking for, stating that its data are obtained from extruded shapes material unless otherwise noted. A molded part adds its own variables again: a part that is injection molded carries weld lines and flow orientation that a machined part cut from stock does not, so the same polymer’s tensile figure reads differently on each.

Reading Tensile Values Before You Specify

A short set of checks makes a sheet usable.

  • Find the word yield or break next to every strength. When it is missing, ask.
  • Find the specimen type and the pull speed. When they are missing, treat the sheet as a typical value for comparison, which several sheets call it.
  • Check whether the sheet cites ASTM D638 or ISO 527, and do not mix the two.
  • Look up the thickness range of the stock the values came from, since thickness above 14 mm means a machined specimen.
  • Compare the modulus and the elongation alongside the strength, because the pair says how far a part moves before it yields.

For shapes made to a material standard, tensile values are part of what the standard asks. The ASTM D6100 abstract for acetal shapes lists tensile strength, elongation at break and tensile modulus among the physical properties a shape has to meet, together with dimensional stability, flexural modulus, Izod impact and porosity level. That edition on astm.org is historical, so a call-out that names D6100 should say which edition it means. Where a drawing needs a tensile figure from a lot, the lot’s own result, tied to the standard that governs the shape, answers the question that a typical value cannot.

Table 3. What a call-out for tensile strength needs
Field Example form Why
Test method and edition ASTM D638-22 the edition names the conditions
Reading tensile stress at yield yield and break differ by factors for ductile grades
Specimen and speed Type I, 5 mm/min the standard says speed and thickness move the number
Condition 23 °C, stated humidity conditioning is part of the scope
Basis typical or minimum, per lot makers print typical values for comparison

A complete line reads like this: tensile stress at yield, ASTM D638-22, Type I specimen, 5 mm/min, 23 °C, typical value from the grade’s maker sheet. Each clause answers one row of Table 3 above, and a supplier who cannot supply one has told the buyer something about the sheet it is quoting from.

For a part where strength decides the design, run in a few hundred pieces, low-volume plastic CNC followed by bridge production gives the buyer parts to load-test on the real geometry, which answers the questions the sheet cannot.

Sources and Further Reading

Request a Plastic CNC Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Plastic CNC chosen.

Request a Quote