A 1,000 mm (39.4 in) acrylic part grows by 1.4 mm when the room warms from 10 °C to 30 °C. Röhm, the maker of PLEXIGLAS, prints that example in its machining guidelines, and it explains why a plastic part clamped hard at both ends can bow before the first chip is cut. The movement is thermal, the clamp turns it into stress, and the stress comes out as shape.
MCAM states the mechanical half of the problem in its 2026 guide: plastics are much more elastic than metals, so a part clamped as tightly as a steel blank deforms under the jaw. A part held too lightly can leave the fixture instead. Every workholding choice on plastic sits between those two failures.
The sections below follow a part through its setup in the order a machinist meets the decisions, with the figures each maker prints and the edition they come from.
How to Hold a Plastic Part on a CNC Machine
Hold it on as much surface as the geometry allows, with the lowest force that keeps it from moving, and with every thin wall backed by something solid. That sentence compresses three recommendations that recur across the stock-shape makers’ guides: light clamping, support under the cut, and distribution of the force by vacuum or soft jaws instead of point contact.
The reasons are the material’s own. Mitsubishi Chemical Advanced Materials (MCAM) lists four differences in its 2026 machining guide: thermal expansion up to ten times that of metals, slower heat loss, much lower softening and melting temperatures, and much higher elasticity. Each one touches the fixture. Expansion moves the part against its stops during the cut, slow heat loss lets a warm spot grow where a jaw touches, a low softening point turns friction into a mark, and elasticity lets the whole blank deflect away from the tool.
Table 1 pairs the common part forms with the holding methods the makers name. The right-hand column carries the condition each source attaches.
| Stock form | Holding method | Condition from the source |
|---|---|---|
| Plate or sheet | Vacuum plate, with surrounds that support the part | MCAM 2026 recommends vacuum plates for plate parts and surrounds on the plate for further support |
| Thin sheet | Flat, solid support under the part; mechanical clamp or vacuum | Röhm, drilling and milling PLEXIGLAS: hold firmly to avoid fluttering or splitting |
| Tube, ring, bushing | Blank pressed into a bored end at the chucked end | MCAM 2026, turning tips: the blank supports the clamp force of the jaws |
| Rod | Collet; fixed-pressure jaws on a new machine | MCAM 2026 names Crawford collets and fixed-pressure jaws |
| Small, long section | Sliding-head lathe | MCAM 2026, turning tips |
| Hard, notch-sensitive grades | Light clamping, chamfered corners, diamond tooling | MCAM 2026 for PBI, PI and MT-01 filled PTFE |
None of these entries is a tolerance claim. Each is the method a maker prints for the shape in the first column.
A plastic part is held by the smallest force that stops it from moving and the largest area that spreads it. Point clamps and tight three-jaw chucks do the opposite on both counts.
Why Clamping Force Shows Up in the Measured Size
Plastic recovers elastically, and the cut happens while it is still squeezed. A bore turned in a ring held by three hard jaws is cut round while the ring is slightly triangular. When the jaws open, the ring relaxes toward its free shape and the bore follows it. The error is invisible on the machine and obvious on the gauge.
MCAM’s tip for tubes is the standard answer: bore one end and press a blank into it, so the jaws press on a solid body and the wall between them and the cut does not collapse. The idea moves the load from the thin wall to a solid member.
Ensinger, another stock-shape maker, adds a stress angle in its frequently asked questions. Its list of advice for machined parts includes avoiding high tensional forces to avoid distortion, and it names blunt or unsuitable tools as a separate source of added stress. A clamp that deforms a part does two jobs wrong: it shifts the cut, and it adds load to a blank that already carries manufacturing stress.
Heat travels through the same path.
Plastics conduct heat poorly, so the energy of a cut stays near the cutting edge and the surface under the jaw. MCAM’s summary page warns about localized overheating. A fixture that pins a hot spot, such as a jaw lying against a recently drilled wall, keeps that region from relaxing evenly. A part warmed by a long drilling cut has to cool completely and uniformly to room temperature before finishing starts, so the holder is not the only thing that waits on the part.
Preparing the Stock Before the First Clamp
The setup starts before the part is on the machine. Four preparations come directly from the makers’ documents.
- Let the stock reach shop temperature. Ensinger notes that products stored in cold conditions should be allowed sufficient time to acclimatize before processing.
- Keep the protective film on. Röhm leaves the masking film on its acrylic sheet during all machining operations and marks out on the film.
- Choose between rod and plate. MCAM’s general rules say to consider rod as well as plate for the same part, because the two forms leave the symmetry of the finished part in different places. Ensinger’s 2024 stock catalog lists its acetal as rods from 3 to 300 mm and plates from 0.5 to 150 mm thick, so either form usually exists in the size the part needs.
- Plan the symmetry. MCAM advises balanced machining on both sides of the shape’s centerline, with pockets on one face balanced by grooves on the opposite face.
The temperature point deserves a table. Röhm gives the linear thermal expansion of PLEXIGLAS GS and XT as 0.07 mm per meter per kelvin; the 1.4 mm in the opening is that coefficient multiplied by 1 m and 20 K. The guide’s own conclusion is to check the dimensions of identical parts at the same ambient and material temperatures. Table 2 scales the coefficient to shorter lengths for a 10 K difference between the stock and the room.
| Length, mm (in) | Change, mm (in) |
|---|---|
| 100 (3.9) | 0.07 (0.003) |
| 250 (9.8) | 0.18 (0.007) |
| 500 (19.7) | 0.35 (0.014) |
| 1,000 (39.4) | 0.70 (0.028) |
Other polymers carry other coefficients, and their makers print them on datasheets. The point of the table is the order of magnitude. A stock block carried from a cold store to the table can move by more than a fine tolerance before the first cut, and a clamp that locks it at both ends turns that movement into a bow.
Holding the Stock While It Is Sawn to Blanks
The first clamp of the job is usually on a saw. A shape that vibrates on the saw table cuts rough or even breaks, so it is clamped firmly for the cut. MCAM says reinforced grades are preferably cut with a band saw of 4 to 6 mm tooth pitch, 2 to 3 mm for PBI, PI and MT-01, and that standard circular saws usually lead to cracks in them.
A blank that is cut badly starts the machining with stress already in it. Fixturing that holds the part firmly is also what lets the cutter run at the table travel and spindle speed plastics want, so a grip that is good enough to hold at speed lets the cutter run in its efficient range. The chain of holds from saw to mill to lathe to measuring table is one system, and each link affects the next.
Vacuum Plates and Surrounds for Plate Parts
Vacuum plates solve the distribution problem for flat stock. Atmospheric pressure presses the entire underside against the table, so no jaw touches the edge. MCAM 2026 recommends vacuum plates for plate parts and describes surrounds, which are raised edges or pins on the plate that support the part further. Röhm describes the same method for acrylic sheet, either clamped mechanically or sucked against the table under vacuum, and insists that in both cases it is held firmly to avoid fluttering or splitting.
Three conditions limit a vacuum hold on plastic, and they are matters of engineering sense more than printed limits. The sealed area has to carry the cutting force, so a part with deep pockets loses grip as the pockets open, and the first operation is usually the one that cuts least into the sealing face. Flatness of the underside matters as well, which means plate that bowed in earlier machining may not seal until a surround or a light first pass flattens it. Chips have to leave: MCAM suggests vacuuming dry chips from milling machines and calls for machines with a cavernous swarf area, because a chip trapped under a part lifts it.
Thin sheet needs a second layer of care. Röhm instructs that thin sheets are clamped onto a flat, solid support for drilling so that the bottom surface does not chip, with a slow feed at the start and again before the bit leaves the underside. A vacuum plate with a sacrificial board on top performs the same function for a milled profile.
On a vacuum plate the part is supported on its whole underside, so the cutter can reach the edge. The price is the sealing area, which every opened pocket reduces.
Marking Out Without Notching the Part
Layout lines are part of holding, because a mark made with the wrong tool becomes a stress concentration. Röhm advises marking out on the masking film, and, once the film is off, with soft lead or grease pencils. Scribers and prick punches are not used unless the notches they cause are removed in a later operation, because otherwise all the materials the guide covers, even impact-modified acrylic, may crack or break under load.
The same logic applies to the datum marks a fixture leaves. A pin, a clamp edge or a punch mark that sits inside a finished surface is a notch, and the hardest grades are the least forgiving. MCAM gives those grades, polybenzimidazole, polyimide and the filled PTFE grade MT-01, their own saw pitch and diamond tooling, and the separate treatment reflects the same notch sensitivity.
Jaws, Collets and Plugs for Rod and Tube
Turned parts meet the same conflict at a smaller scale. A rod is gripped on its outside, and the grip has to be firm enough to transmit torque from a cut that can run at hundreds of meters per minute. MCAM 2026 prints cutting speeds of 200 to 500 m/min for polyamide, acetal and UHMW-PE turning, which are values for the cut, not the grip, but they show how much torque the holder carries.
MCAM’s tips for turning give four holding ideas:
- Use collets. The guide says Crawford collets work very well for plastic.
- On a new machine, consider fixed-pressure jaws, so the grip does not depend on operator feel.
- For tubes, bore one end and place a blank inside to support the jaw force.
- For small, long sections, use a sliding-head machine, which supports the bar close to the cut.
Support matters as much as force. Work that is not supported deflects under the cut, and a bushing held only at its thin wall comes out of round. For the hard and moderately tough grades, such as PBI, PAI, PI, glass-filled or carbon-filled PEEK, and filled PPS, the hold is light and the part is never forced into the fixture.
One more habit comes from the MCAM turning tips: most diameters grow after cutting, so the setting aims for the lowest dimension in the band. A machinist who knows the grip is light can trust that growth to be the material’s own, and can offset for it with fewer surprises.
Holding the Part for the Second Side and the Rest Between Cuts
A plate part usually needs two setups, and the second one is where distortion shows. When the first operation removed material from only one face, the blank has released stress on that side. Asymmetric or heavy section changes, for example a U-shape machined from a plate, release internal stress and can deform the part. The remedy is balanced machining on both sides of the stock centerline, or an anneal after pre-machining.
MCAM states the same idea as a numbered solution set for extrusions that bow after one-sided machining. The advice is to start with the thickest plate, move the extrusion centerline away from the machined features, machine slots or grooves on the opposite face, and balance the cuts on both sides. In the turning tips it adds a time instruction: for improved tolerances, rough out large sections and leave them for 24 hours. The fixture for the second side has to take the roughed part in its relaxed shape. Measuring the flatness of the rested part before it is clamped tells whether it bowed; a part that bowed by a fifth of a millimeter (0.008 in), as an illustration, will be pulled flat by a vacuum plate or a vise, cut flat, and spring back by about the same amount when released. The finishing pass is therefore taken at light depth. MCAM says that after rough machining and annealing, flatness improves with a very light finishing cut.
A part that goes into an oven between roughing and finishing is fixtured during the whole annealing cycle, and MCAM adds that it stays fixtured until it has cooled slowly to the touch. Annealing itself has its own piece in these resources; the point here is that the holder does not end at the machine.
Reading the Signs That a Part Was Held Wrong
Stock-shape makers publish troubleshooting charts, and several columns point to workholding. Table 3 lists the symptoms for which MCAM’s turning chart names support or sharp corners as a cause, alongside the other causes it prints, so a reader can separate the fixture from the tool.
| Symptom | Causes in the chart that involve the fixture | Other causes in the same column |
|---|---|---|
| Chatter | Tool not mounted solidly; material not supported properly | Dull tool, tool below center, too much nose radius, depth of cut too heavy |
| Burrs at the edge of the cut | No chamfer at sharp corners, so the tool meets full edge thickness at once | Dull tool, insufficient side clearance |
| Chipping of corners | None named; a tool eased into the cut gradually lowers the shock the hold has to take | No lead angle, too much positive rake, tool not eased into the cut |
Beyond the chart, a few observations separate holding errors from tool errors. A pattern of chatter marks that follows a thin wall points to support, not to cutting speed. Bores that measure round on the machine and oval on the gauge point to clamp deformation. A part that is flat when it comes off the table and bowed after a day points to released stress, which the second-side practice above addresses.
Design helps here as well. MCAM lists a missing chamfer at sharp corners among the causes of cracked and chipped corners, and a radius or chamfer gives the tool a gradual entry and exit, which reduces the shock load that a marginal hold cannot take.
A Setup Order for a Machined Plastic Part
Putting the pieces in sequence, a stock-shape maker’s guidance reads as a short procedure:
- Bring the stock to shop temperature and leave masking film in place.
- Choose rod or plate so that the finished part is symmetrical about the stock centerline, or plan opposite-face grooves to balance pockets.
- Hold plate on a vacuum plate with surrounds, and tube or ring on a plug or soft support, with light force.
- Rough with oversize, support the part, and rest it for the time the maker recommends.
- Re-fixture on the relaxed shape and finish with a light cut.
- Deburr with tools that do not cut too deep, then measure at a controlled temperature.
Each step moves a failure from the final dimension, where it costs a part, to an earlier stage, where it costs minutes.
For buyers weighing a first run, the drawing carries its own holding decisions: a flat datum face for the vacuum plate, a symmetrical stock layout, radii in internal corners and a note on which faces are critical. Parts that arrive with those decisions already visible need fewer re-fixtures, because the holder can be designed with the part instead of after the first one fails, and that holds for low-volume plastic CNC as it does for bridge production.
Sources and Further Reading
- Mitsubishi Chemical Group, Mitsubishi Chemical Advanced Materials, Guide to machining plastic parts, metric edition, 2026
- Ensinger, Frequently asked questions, machinable plastics
- Ensinger, Stock Shapes catalog, 2024, TECAFORM AH stock sizes
- Röhm, Guidelines for workshop practice, Machining PLEXIGLAS