An 8 mm (0.31 in) end mill turning at 11,000 rpm cuts acrylic at about 276 m/min. Röhm, the maker of PLEXIGLAS, names that exact pairing as a good result in its machining guidelines, and the surface speed is nowhere near what the same cutter would see in steel. The figure sits inside a recommended band of 200 to 4,500 m/min for milled acrylic, which is so wide that it hides the real constraint: the spindle may go as fast as the machine allows, but the heat has to go somewhere, and a plastic offers the cutter only one exit.
That exit is the chip. Plastics conduct heat poorly and soften at temperatures where metals are still cold, so the whole discipline of cutting them comes down to making each chip big enough, sharp enough and fast enough to carry the heat away before the part absorbs it. The sections below follow that idea through tool material, geometry, milling, turning, drilling and coolant, with every figure tied to the maker and the edition that printed it.
Tool, Speed and Feed for CNC Plastic Machining
Use a sharp tool with generous clearance, a feed rate as high as the surface allows, and a path that lets the chip leave. That is the common opening of the stock-shape guides. Mitsubishi Chemical Advanced Materials (MCAM) lists five working rules in its 2026 guide: keep tools sharp and smooth, run feeds as high as possible, give the cutting edge enough clearance that only the edge touches the plastic, remove the swarf from the tool, and apply coolant where a lot of heat is generated, such as drilling.
The second layer is material specific. A cast polyamide or an acetal cuts in a way that a glass-filled PEEK or a polyimide does not, and the guides sort polymers into families with different tool recommendations. The speeds are given as surface speed in meters per minute and feed in millimeters per revolution or per tooth. Metric first, inches follow where they help: 200 m/min is 656 ft/min, and 0.5 mm/rev is 0.020 in/rev.
Ensinger, another stock-shape maker, frames the same preference more bluntly. Its answer to what affects machinability is that commercial wood and metalworking machines work with HSS tools, but tools with a sharper wedge angle than the ones used for aluminum are recommended, and reinforced plastics are not for hardened steel tools, because of the short tool life. Tungsten carbide, ceramic or diamond tipped tools are advised there.
Cutting plastic is a heat-removal problem with a geometry attached. A dull tool, a slow feed and a clogged flute all fail the same way, by leaving the heat in the part.
Where the Heat Goes When Plastic Is Cut
MCAM puts the central skill in one line: because of poor thermal conductivity and lower melting properties, the job is to avoid heat build-up and to evacuate swarf, which avoids deformation, stress build-up or even melting. MCAM’s summary of plastics versus metals lists the consequences: heat loss is slower, localized overheating has to be avoided, and the softening and melting temperatures are much lower. Ensinger states the design rule in one line: the best form of cooling is heat dissipation through the chips produced.
Three practical effects follow from that rule:
- A feed that is too low shaves a thin chip that carries little heat, and the tool rubs. MCAM’s turning chart lists feed too slow and spindle speed too fast as causes of a melted surface.
- A feed that is too high tears the material. Röhm’s drilling pictures show that speed or feed too high gives a crumbly chip and an uneven cut, speed or feed too low gives a molten chip, and a smooth continuous chip marks the right pair.
- A part that heats unevenly relaxes unevenly. Heat input appears in Ensinger’s list of dimensional-stability factors alongside moisture uptake and stress relaxation, and the same page notes that semi-crystalline thermoplastics show post-shrinkage of up to about 1.0 to 2.5 percent, with amorphous ones at about 0.3 to 0.7 percent.
The continuous chip is therefore a sign, not just a nuisance. Röhm calls a continuous chip flow proof of the correct grinding angle, feed rate and cutting speed, in turning as in drilling. A buyer reading a shop’s sample part can use the same sign: a clean, shiny, uniform surface came from a chip that left in one piece.
Tool Material and Geometry by Polymer Family
This table collects the turning data MCAM prints for its stock shapes in the 2026 edition. The first column lists a family by the grades named in the guide. Each value is a recommended range from the guide, and no shop is bound by it.
| Family (grades named by MCAM) | Rake angle, degrees | Feed, mm/rev (in/rev) | Cutting speed, m/min (ft/min) | Tool |
|---|---|---|---|---|
| Polyamide, UHMW-PE | 0 to 10 | 0.05 to 0.5 (0.002 to 0.020) | 200 to 500 (656 to 1,640) | HSS or carbide |
| Acetal (POM-C, POM-H) | 0 to 10 | 0.05 to 0.5 (0.002 to 0.020) | 200 to 500 (656 to 1,640) | HSS or carbide |
| PET-P, unfilled PEEK, PAI T4203 | 0 to 10 | 0.05 to 0.5 (0.002 to 0.020) | 200 to 400 (656 to 1,312) | Carbide |
| PC, PPSU, PEI, PSU | 0 to 10 | 0.05 to 0.4 (0.002 to 0.016) | 200 to 400 (656 to 1,312) | Carbide |
| Glass or carbon reinforced polyamide, PAI, PEEK and PPS | 0 to 10 | 0.05 to 0.3 (0.002 to 0.012) | 100 to 200 (328 to 656) | Carbide or PCD/CVD |
| PBI, PI, PTFE with filler MT-01 | 3 to 5 | 0.05 to 0.2 (0.002 to 0.008) | 25 to 100 (82 to 328) | Carbide or PCD/CVD |
| Filled PTFE, other grades | 0 to 5 | 0.05 to 0.4 (0.002 to 0.016) | 150 to 400 (492 to 1,312) | Carbide |
Reading down the table, the speed and the feed fall as the material gets harder or more abrasive, and the tool changes from HSS to carbide to diamond. The relief angle in the guide is 5 to 15 degrees for all families except filled PTFE, where it narrows to 8 to 12 degrees.
Other makers print different columns for the same job. Röhm gives rake 0 to minus 4 degrees, relief 5 to 10 degrees and a cutting edge angle near 45 degrees for turning acrylic, with 20 to 300 m/min, feed 0.1 to 0.5 mm/rev and cutting depth up to 6 mm. It also recommends tool bit radii of at least 0.5 mm, and notes that carbide is suitable for roughing while HSS is usually used for the finishing pass. MCAM points to 0.8 mm radius as the best finish, and to inserts designed for non-ferrous metals such as aluminum or brass.
A datasheet value from one maker is not a recipe for a different grade from another. The guides are specific to the stock shapes their makers sell, and they print this disclaimer themselves. Treat the table as a map of ranges; a program for a real part starts from the grade’s own datasheet.
Milling Plastic With Climb Cuts and Open Flutes
Milling raises the same question as turning with an extra complication: the cutter goes in and out of the material many times per second. MCAM’s milling advice is short. Use milling cutters with fewer teeth, a higher helix and good clearances; leave plenty of swarf area; avoid conveyor chip removal; and consider vacuuming dry chips. MCAM recommends climb milling over conventional milling, since it gives a smaller break, less heat and a better finish.
The pictures of climb and conventional milling in the MCAM guide read as follows. In a climb cut, the tooth enters at full chip thickness and leaves at zero, so the break is small, the heat is lower and the finish is better. A conventional cut starts the tooth at zero thickness, rubs before it bites, and leaves with a large break, which gives more heat and a worse finish.
Röhm adds a point on flute count for high-speed trimming of acrylic. Single or double-fluted end mills with good chip removal are used for small diameters to reach high cutting speeds, and multiple-fluted cutters at high speed are likely to clog. A single flute also needs a balanced chuck, because an unbalanced spindle leaves chatter marks and can damage the machine. The cutting data Röhm prints for the cutter is rake 0 to 5 degrees, relief 2 to 10 degrees, up to 6 mm cutting depth and feed up to 0.5 mm/rev.
The milling data of MCAM, in feed per tooth, follow the same family order as the turning data. Polyamide and UHMW-PE take up to 0.5 mm per tooth at 200 to 500 m/min with HSS or carbide.
Acetal takes up to 0.5 mm per tooth at 200 to 400 m/min. Unfilled PEEK and PET-P drop to 0.4 mm per tooth at 150 to 300 m/min with carbide. Reinforced grades run at 0.3 mm per tooth and 75 to 150 m/min, and PBI, PI and the filled PTFE grade MT-01 at 0.15 mm per tooth and 25 to 100 m/min.
Sawing the Blank Before the Cut
Sawing comes before any CNC operation, and the guides give it numbers. MCAM’s sawing table lists band saw cutting speeds of 50 to 500 m/min (164 to 1,640 ft/min) and tooth pitch of 4 to 10 mm (0.16 to 0.39 in) for polyamide, acetal and the unfilled PEEK and PET-P grades, and pitch of 2 to 3 mm (0.08 to 0.12 in) at 25 to 100 m/min for PBI, PI and the filled PTFE grade MT-01. Reinforced grades take a 4 to 6 mm pitch.
MCAM says that reinforced materials are preferably cut with a band saw and not a circular saw, because circular saws usually lead to cracks. The tooth set has to be wide enough that the kerf does not close behind the blade, and soft low-temperature materials need a coarse pitch while filled and thinner stock needs a finer one. A blank sawn with these rules reaches the machine without heat damage on its faces.
Turning and Parting Plastic Rod
Turning produces the longest chips of any operation, and a continuous stream of stringy plastic wraps around the chuck, the tool and the part. MCAM recommends a compressed air powered suction system for turning and boring, which sends the swarf directly into a container, and adds that machines should have a cavernous area for swarf and no conveyor belts.
Parting off has its own troubleshooting chart in the MCAM guide. It names a dull tool, insufficient side clearance and insufficient coolant supply as causes of a melted surface, and it lists a chamfer applied before the cut-off among the remedies for burrs at the cut-off point. The shared fix is a sharp tool on center with enough clearance.
Threading in plastic is a gentler version of metal work. MCAM says tools do not have to be as rigid as metal cutting tools. Single-point threading with a sharp insert and light final passes keeps the flanks clean. For tapped holes, MCAM suggests spiral taps, rigid-tap cycles on the CNC and a check of the pilot drill size, because most plastics close up after drilling, which makes taps tight. For thread inserts, MCAM calls self-tapping inserts the most popular but asks for caution, and for a check that the hole has not closed after insertion.
Drilling Deep Holes Without Cracking or Melting
Drilling is the operation where plastic punishes shortcuts, and the rules are well settled. MCAM says plastics build up heat very easily in drilling, especially when hole depths are greater than twice the diameter, so a cooling liquid is generally recommended. Frequent pull-outs, or peck drilling, improve heat and swarf removal.
Table 2 summarizes the drilling rules stated across the three guides, split by hole size.
| Condition | Rule | Source |
|---|---|---|
| Small holes, 0.5 to 25 mm (0.02 to 1 in) | HSS twist drill, peck drilling, slow spiral (low helix) drill | MCAM 2026 |
| Holes of 25 mm (1 in) and larger | Drill with thinned web; drill stepwise, for example 12 mm then 25 mm for a 50 mm bore, then bore | MCAM 2026 |
| Drill point, general data | Top angle 90 to 120 degrees, relief 5 to 10 degrees, rake 3 to 5 degrees, feed 0.1 to 0.3 mm/rev, speed 50 to 100 m/min for most families | MCAM 2026 |
| PBI, PI, MT-01 filled PTFE | Speed 25 to 50 m/min, carbide or PCD/CVD | MCAM 2026 |
| Solid pieces | Insert drill with the right inserts | MCAM 2026 |
Thinned web, slow spiral and a pull-out at about 1.5 diameters leave the heat in the chips. Pushed straight through, a drill leaves it in the wall of the hole.
A part drilled warm and finished warm will change size as it cools, so a part heated by a long drilling cut is left to reach room temperature, uniformly through the section, before finishing starts.
Cracks are the failure that matters most on the hard grades, and they start as microcracks from a grabbing drill. A steady machine feed avoids that, and a two-step drill-and-bore method suits notch-sensitive materials: an insert drill removes most of the material, then a boring bar finishes the bore so that the final dimension comes from a gentle cut.
Coolant and Stress Cracking in Amorphous Plastics
Most machining of thermoplastics runs dry or with air. MCAM says coolants are generally not required for most operations, apart from drilling and parting off. When a shop wants the best finish and the closest tolerance, it suggests nonaromatic, water-soluble coolants, spray mists or pressurized air, which cool the interface and blow chips from the cut.
The exception is the amorphous family: polycarbonate, PSU, PPSU and PEI, listed by name in MCAM’s guide. These grades are susceptible to environmental stress cracking, and petroleum based cutting fluids and many water-soluble coolants can start it. The recommended coolants for them are pure water or compressed air.
If a coolant cannot be avoided, for example in deep holes or tapping, the part is cleaned immediately with isopropyl alcohol and rinsed with pure water. MCAM also notes one product, a flame-retardant UHMW-PE grade, as dry machining only, with compressed air or air spray as the only cooling, since its additives can react with liquids and corrode tooling.
Röhm’s guidance for acrylic is compatible: a drilling emulsion or cutting oil compatible with acrylic can cool turning cuts, though cooling is not recommended for precision work with diamond tools because it causes optical flaws on high-gloss surfaces.
Water has one more role that is easy to forget. A 2018 study by Mustafa Bozdemir of Kırıkkale University on end milling of cast polyamide PA6G tested humid and dry plates with carbide and HSS tools, and records that the material is vulnerable to humidity up to 7 percent. The study varied cutting speed, feed, cutter diameter and depth and then modeled surface roughness. Its conclusion is about prediction accuracy, not a new rule, but the choice of humid and dry samples as an input shows that the state of the stock is a variable alongside the cut.
Reading the Surface Back Into the Program
Once a part is cut, the surface tells the programmer what to change. Table 3 pairs the most frequent defects with the causes MCAM prints for turning and boring, so that a rough or melted surface can be traced to a parameter and not blamed on the grade.
| Defect | First causes to check |
|---|---|
| Melted surface | Dull tool or heel rubbing, insufficient side clearance, feed too slow, spindle speed too fast |
| Rough finish | Feed too heavy, incorrect clearance angles, sharp point on the tool where a slight nose radius is needed, tool not mounted on center |
| Burrs at the edge of the cut | No chamfer at sharp corners, dull tool, insufficient side clearance |
| Chipping of corners | No lead angle, too much positive rake, tool not eased into the cut |
| Chatter | Dull tool, tool below center, too much nose radius, tool not solid, work not supported, depth of cut too heavy |
The pattern is that a melted surface and a rough surface are opposite errors in feed, and the program changes in opposite directions. A melted surface asks for a higher feed and a lower spindle speed; a rough surface asks for a lighter feed and a better nose radius. MCAM’s turning tips add a polishing step for grind marks, using hand diamond tools, and suggest sharpening the top face of an insert to improve the front edge.
For a buyer, the practical use of this chart is to ask for the conditions behind a sample, not only its dimensions. Four answers describe a controlled cut:
- the tool material and its edge condition at the start of the run;
- the surface speed and the feed, in meters per minute and millimeters per revolution or per tooth;
- the chip type, continuous or broken, and how it was removed;
- the coolant or air used, and the cleaning step after it for amorphous grades.
A shop that can state them has written down its process, and the same parts keep the same finish and dimensional behavior when the work moves between machinists or from a first run to a longer one. Planning low-volume plastic CNC next to bridge production depends on that record.
Sources and Further Reading
- Mitsubishi Chemical Group, Mitsubishi Chemical Advanced Materials, Guide to machining plastic parts, metric edition, 2026
- Ensinger, Frequently asked questions, machinable plastics
- Röhm, Guidelines for workshop practice, Machining PLEXIGLAS
- Mustafa Bozdemir, Prediction of surface roughness considering cutting parameters and humidity condition in end milling of polyamide materials, PMC6046151